ASA and ABS are close cousins, and confusing them is one of the most common and most expensive material selection errors in plastics. This guide explains the difference mechanistically and gives the selection rules.
1. The Structural Difference
| Aspect | ABS | ASA |
| Full name | Acrylonitrile butadiene styrene | Acrylonitrile styrene acrylate |
| Matrix | SAN (styrene-acrylonitrile) | SAN (styrene-acrylonitrile) |
| Rubber phase | Polybutadiene | Acrylate rubber |
| Rubber backbone | Unsaturated (contains C=C double bonds) | Saturated (no double bonds) |
| UV vulnerability | High — double bonds are the attack site | Low — no primary attack site |
| Glass transition of rubber | About −80 °C | About −40 °C |
| Low-temperature toughness | Better | Moderate |
| Weathering | Poor | Excellent |
| Relative cost | $ | $$ |
The matrix is identical, and that is why the mechanical properties are so similar. Both polymers are styrene-acrylonitrile copolymer with a dispersed rubber phase that provides toughness. Because the continuous phase — the part that carries most of the load — is chemically the same, tensile strength, modulus, and hardness are nearly identical between ABS and ASA.
The rubber phase is where they diverge, and it controls both toughness and weathering. Polybutadiene’s backbone contains carbon-carbon double bonds, which are chemically reactive and are precisely the site that UV radiation attacks. Acrylate rubber has a saturated backbone with no such double bonds, so there is no primary site for UV-induced chain scission.
| Structural Feature | Consequence |
| Same SAN matrix | Nearly identical strength, modulus, hardness |
| Different rubber | Different weathering, different low-temperature toughness |
| Polybutadiene’s double bonds | UV attack site → yellowing, embrittlement |
| Acrylate’s saturated backbone | UV resistant → color and impact retention |
2. Property Comparison
| Property | ABS | ASA | Test Standard |
| Density (g/cm³) | 1.04–1.07 | 1.05–1.07 | ISO 1183 |
| Tensile strength (MPa) | 40–50 | 40–50 | ISO 527 |
| Tensile modulus (MPa) | 2,000–2,400 | 2,000–2,300 | ISO 527 |
| Elongation at break (%) | 15–30 | 20–35 | ISO 527 |
| Flexural modulus (MPa) | 2,000–2,400 | 2,000–2,300 | ISO 178 |
| Notched Izod, 23 °C (kJ/m²) | 15–30 | 10–20 | ISO 180 |
| Notched Izod, −20 °C (kJ/m²) | 8–15 | 5–9 | ISO 180 |
| HDT at 1.8 MPa (°C) | 90–100 | 90–100 | ISO 75-2 |
| Vicat softening (°C) | 100–110 | 100–110 | ISO 306 |
| Rockwell hardness | R100–R110 | R95–R105 | ASTM D785 |
| Mold shrinkage (%) | 0.4–0.7 | 0.4–0.7 | ISO 294-4 |
| Water absorption, 24 h (%) | 0.2–0.3 | 0.2–0.3 | ISO 62 |
| Gloss | High | High | — |
| UV resistance | Poor | Excellent | — |
Most rows are the same, and that is the point. Strength, modulus, heat deflection, Vicat, hardness, shrinkage, and water absorption are effectively identical. If you compare two data sheets side by side, you will find very few differences in the standard mechanical table.
The meaningful mechanical difference is impact, and it favors ABS. ABS’s notched Izod of 15–30 kJ/m² is roughly 1.5 times ASA’s 10–20 kJ/m², and the gap widens at low temperature because polybutadiene’s glass transition is about −80 °C against the acrylate rubber’s −40 °C. That means ABS stays tough down to lower temperatures, while ASA’s toughness begins to fall off at around −40 °C.
| Property | Advantage |
| Room-temperature impact | ABS |
| Low-temperature impact | ABS |
| Tensile strength | Comparable |
| Stiffness | Comparable |
| Heat resistance | Comparable |
| Weathering | ASA |
| Color retention | ASA |
| Indoor cost | ABS |
3. Weathering: The Deciding Difference
| Exposure | ABS | ASA |
| QUV 500 h color shift (ΔE) | 3–6 | <1 |
| QUV 1,000 h color shift (ΔE) | 6–12 | 1–2 |
| QUV 2,000 h color shift (ΔE) | 12–20 | 2–3 |
| Gloss retention after 2,000 h | 30–50% | >85% |
| Impact retention after 2,000 h | 30–50% | >80% |
| Unstabilized outdoor life | 0.5–2 years | 10+ years |
| Stabilized outdoor life | 2–4 years | 10+ years |
A ΔE of about 3 is the threshold of perceptibility. ABS crosses it within 500 hours of accelerated exposure and is well beyond it by 1,000 hours, while ASA stays under it through 2,000 hours and beyond.
Impact loss follows the color change, and it is the more serious failure. A yellowed part is an appearance problem; an embrittled part is a functional failure. ABS’s impact strength falls by half or more over the same exposure that leaves ASA’s essentially intact, because the UV-induced chain scission in the polybutadiene destroys the rubber’s ability to absorb energy.
The mechanism explains why UV stabilization cannot close the gap. A UV absorber works by intercepting photons before they reach the polymer and dissipating the energy as heat. But polybutadiene’s degradation is a chain reaction: once an oxidative chain begins, it propagates. A UV absorber reduces the initiation rate but cannot stop the propagation. ASA has no double bonds to initiate that chain, so there is nothing for a stabilizer to prevent.
| Exposure Condition | ABS | ASA |
| Direct sun, moderate climate | 0.5–2 years | 10+ years |
| Direct sun, high UV | Under 1 year | 8–12 years |
| Behind glass, indoor | Years | Decades |
| Fully indoor, no daylight | Indefinite | Indefinite |
| Fluorescent lighting, indoor | Slow yellowing | Minimal |
| Shaded outdoor | 2–5 years | 10+ years |
Even indoor exposure can matter. Fluorescent and LED lighting emit small amounts of UV, and a part under continuous fluorescent light — a display housing, a light fixture component — will yellow slowly if made from ABS. ASA resists this, which is why some indoor applications specify ASA despite the higher cost.
4. Impact and Low-Temperature Performance
| Temperature | ABS Notched Izod (kJ/m²) | ASA Notched Izod (kJ/m²) | Winner |
| 23 °C | 15–30 | 10–20 | ABS |
| 0 °C | 10–20 | 8–14 | ABS |
| −20 °C | 8–15 | 5–9 | ABS |
| −30 °C | 6–10 | 3–6 | ABS |
| −40 °C | 4–8 | 2–4 | ABS |
ABS is the tougher material at every temperature. The polybutadiene rubber’s much lower glass transition (−80 °C versus −40 °C) means it remains rubbery and energy-absorbing far below the temperatures at which ASA’s acrylate rubber stiffens.
But this advantage is lost outdoors. After UV exposure, ABS’s impact strength collapses — a two-year-old outdoor ABS part may have less remaining toughness than a new ASA part. The comparison that matters in service is degraded ABS against intact ASA, and there ASA wins decisively.
| Comparison | Winner |
| New ABS vs new ASA, room temperature | ABS |
| New ABS vs new ASA, low temperature | ABS |
| Aged ABS vs aged ASA, outdoors | ASA |
| Aged ABS vs new ASA, outdoors | ASA |
| Aged ABS vs aged ASA, indoors | ABS (no aging) |
Design for the aged condition, not the new one. If a part will be outdoors for its service life, the material’s properties after weathering are what matter to the design. Comparing a new ABS data sheet against a new ASA data sheet in an outdoor application compares the wrong numbers.
5. Where Each Material Is Used
| Application | Material | Reason |
| Indoor appliance housing | ABS | No UV, cheaper |
| Indoor electronics enclosure | ABS | Cost |
| Toy components | ABS | Cost, toughness |
| Indoor automotive trim | ABS | Cost |
| Automotive interior | ABS | No UV, toughness |
| Automotive exterior trim | ASA | UV, color retention |
| Outdoor signage | ASA | UV, gloss retention |
| Outdoor furniture | ASA | UV, durability |
| Garden and lawn products | ASA | UV, color |
| Building profile and siding | ASA | Long outdoor life |
| EV charger housing | ASA or PC/ASA | UV plus structure |
| Roofing and window profiles | ASA | Decade-scale durability |
| Window near daylight | ASA or ASA-capped | UV from daylight |
| Display housing, lit | ASA | Fluorescent UV |
The pattern is entirely driven by UV exposure. Indoor parts are ABS; outdoor parts are ASA; and parts that see daylight through a window are a judgment call that often favors ASA.
Coextrusion is the compromise position. A coextruded profile with an ABS or PVC core and a thin ASA cap layer gets ASA’s weathering at the surface while using cheaper material in the bulk. This is standard practice in building profiles, siding, and automotive extrusions, and it captures most of ASA’s benefit at a fraction of the cost of solid ASA.
| Approach | Weathering | Cost | Used In |
| Solid ABS | Poor | Lowest | Indoor parts |
| ASA-capped ABS | Excellent | Low–moderate | Profiles, siding |
| ABS with UV package | Moderate | Low | Mild outdoor |
| Solid ASA | Excellent | Higher | Exterior parts |
| PC/ASA | Excellent plus impact | Highest | Structural exterior |
6. Cost Structure
| Cost Element | ABS | ASA |
| Pellet price (relative) | 1.0× | 1.3–1.6× |
| Processing cost | Comparable | Comparable |
| Processing temperature | 220–250 °C | 230–260 °C |
| Drying requirement | 2–3 h at 80–90 °C | 2–3 h at 80–90 °C |
| Mold temperature | 50–80 °C | 60–90 °C |
| Cycle time | Comparable | Comparable |
| Total cost for indoor use | Lower | Higher, unjustified |
| Total cost for outdoor use | Higher over life | Lower over life |
ASA costs roughly 30–60% more than ABS per kilogram, reflecting the cost of the acrylate rubber versus polybutadiene. Processing is otherwise similar, so the cost difference is essentially a material cost difference.
Indoors, that premium buys nothing. With no UV exposure, ASA’s weathering advantage is worthless, and ABS’s slightly better impact strength and lower price make it the better choice. Specifying ASA for an indoor part is paying for a property the part will never use.
Outdoors, the premium pays for itself quickly. An ABS part replaced every one to two years — including the labor to replace it, and any service interruption — costs far more over a decade than a single ASA part. The comparison is cost per year of service, not cost per kilogram.
| Scenario | Recommendation |
| Indoor, no UV | ABS |
| Indoor, fluorescent lighting | ASA or ABS with UV package |
| Outdoor, short service life | ABS with UV package |
| Outdoor, permanent | ASA |
| Outdoor, large profile | ASA-capped ABS |
| Outdoor, needs impact plus UV | PC/ASA |
| Cost-critical, no UV | ABS |
7. Processing Comparison
| Parameter | ABS | ASA |
| Drying temperature (°C) | 80–90 | 80–90 |
| Drying time (h) | 2–3 | 2–3 |
| Target moisture (%) | <0.1 | <0.1 |
| Melt temperature (°C) | 220–250 | 230–260 |
| Mold temperature (°C) | 50–80 | 60–90 |
| Injection pressure (MPa) | 60–100 | 70–110 |
| Shrinkage (%) | 0.4–0.7 | 0.4–0.7 |
| Regrind tolerance | Good | Good |
| Plating | Excellent | Poor |
| Painting | Good | Good |
| Welding (solvent) | Good | Good |
Processing is nearly interchangeable, which is one reason a switch from ABS to ASA is often straightforward. Both dry similarly, process at similar temperatures, and shrink similarly, so a mold designed for ABS will usually run ASA with modest adjustment — typically a higher melt and mold temperature.
The one significant processing difference is plating. ABS is the standard substrate for electroplating because the polybutadiene can be chemically etched to create mechanical keying for the metal layer. ASA’s saturated rubber does not etch the same way, so ASA is not a plating substrate. If the part requires plating, ABS is the answer regardless of the UV requirement.
| Process | ABS | ASA |
| Injection molding | Excellent | Excellent |
| Extrusion | Excellent | Excellent |
| Thermoforming | Excellent | Good |
| Electroplating | Excellent | Not suitable |
| Painting | Good | Good |
| Laser marking | Good | Good |
| Solvent bonding | Good | Good |
| Ultrasonic welding | Good | Good |
| Regrind | Good | Good |
Thermoforming slightly favors ABS, which has a wider processing window and greater toughness in the rubbery state. For deep-drawn parts, ABS is more forgiving.
8. Substitution Guidance
Switching from ABS to ASA:
| Consideration | Effect |
| Weathering | Dramatically improved |
| Color retention | Dramatically improved |
| Impact at room temperature | Reduced 20–40% |
| Low-temperature impact | Reduced |
| Cost | Increased 30–60% |
| Processing | Minor temperature adjustment |
| Plating | Not possible |
| Tooling | Usually reusable |
Switching from ASA to ABS:
| Consideration | Effect |
| Cost | Reduced 30–60% |
| Weathering | Lost — outdoor life falls to 1–3 years |
| Impact | Improved |
| Plating | Now possible |
| Risk | Appearance and impact failure outdoors |
| Check | Method | ABS Acceptance | ASA Acceptance |
| MFR / MVR | ISO 1133 | Per grade | Per grade |
| Tensile strength | ISO 527 | Per grade | Per grade |
| Notched Izod, 23 °C and −20 °C | ISO 180 | Per grade | Per grade |
| HDT | ISO 75-2 | Per grade | Per grade |
| Density | ISO 1183 | Confirm grade | Confirm grade |
| Color | Spectrophotometer | Within tolerance | Within tolerance |
| Weathering | QUV on a molded plaque | If required | If required |
| Rubber identification | FTIR or DSC | Confirms butadiene | Confirms acrylate |
| Moisture | Loss on drying | <0.1% | <0.1% |
Rubber-phase identification distinguishes ABS from ASA reliably. FTIR shows the characteristic polybutadiene absorption in ABS that is absent in ASA, and DSC reveals the rubber glass transition at about −80 °C for ABS versus about −40 °C for ASA. This matters because the two look and feel similar, and a substitution would otherwise go unnoticed until the part failed outdoors.
Weathering testing on your own plaque is the decisive qualification. Since weathering is the entire reason to choose ASA, a QUV run on a plaque molded from the actual lot, in the production color, confirms both the material and the process. For an outdoor part with an appearance warranty, this is the most valuable single test.
9. Decision Procedure
Step 1 — Will the part see direct sunlight?
- Yes, permanently → ASA (or PC/ASA for structural parts).
- Yes, short-term or disposable → ABS with a UV package may suffice.
- No → continue.
Step 2 — Will it see daylight through glass, or continuous strong lighting?
- Yes → ASA, or ABS with a UV package as a compromise.
- No → continue.
Step 3 — Is electroplating required?
- Yes → ABS. ASA cannot be plated.
- No → continue.
Step 4 — Is low-temperature impact critical?
- Yes, and the part is indoors → ABS.
- Yes, and the part is outdoors → PC/ASA.
- No → ABS for indoor, ASA for outdoor.
| Scenario | Recommendation |
| Indoor appliance housing | ABS |
| Automotive interior | ABS |
| Electroplated part | ABS |
| Automotive exterior trim | ASA |
| Outdoor signage | ASA |
| Garden products | ASA |
| Building siding and profiles | ASA-capped ABS |
| Outdoor structural housing | PC/ASA |
| Display housing under lighting | ASA |
10. Next Steps
For the ASA versus ABS decision, the sequence is: direct sunlight → ASA; daylight through glass or strong lighting → ASA or stabilized ABS; electroplating → ABS; otherwise → ABS. Low-temperature impact and toughness favor ABS; everything to do with weathering favors ASA.
We supply both ASA and ABS in general-purpose, high-impact, UV-stabilized, and flame-retardant grades, with weathering data and coextrusion support.
[Ask for a Material Recommendation →]
Related Reading
- ASA Plastic: The Complete Guide to Properties and Applications
- ASA vs PVC vs PMMA: Choosing for Outdoor Profiles and Panels
- Is ASA UV Resistant? Weathering Data and Outdoor Service Life
- PC/ASA vs PC/ABS vs ASA: Weathering and Cost Compared
- MABS Plastic: Transparent ABS Explained — Properties and Uses