“PC/ABS alloy” and “PC/ABS blend” refer to the same material, but the word “alloy” is often used to signal a compatibilized, tightly specified blend rather than a simple mechanical mix. That distinction matters commercially: a properly compatibilized alloy at 60:40 can outperform an uncompatibilized blend at 65:35 on impact strength while costing less. This guide covers the alloy’s property profile, its application map, and how to run it on an injection molding machine.
The alloy earns its place for a structural reason. PC alone is tough and heat-resistant but stiff in the melt and expensive; ABS alone flows beautifully and costs little but lacks toughness and heat resistance. Blending them lets a designer trade along a continuous spectrum rather than choosing between two fixed points — and because the ratio, compatibilizer, and additive package can all be tuned, a compounder can deliver a material matched to a specific part rather than the nearest catalog grade. That tunability is the alloy’s real commercial value, and it is also why specification discipline matters so much: the material is only as good as the specification behind it.
1. What Makes It an “Alloy” Rather Than a Blend
PC and ABS are only partially miscible. Left to themselves, they form a two-phase system with poor interfacial adhesion — the ABS domains can debond from the PC matrix under stress, producing brittle failure. A true alloy adds a compatibilizer (typically a SAN-based copolymer or a grafted rubber) that sits at the phase boundary and bonds the two polymers together.
| Feature | Simple Blend | Compatibilized Alloy |
| Interfacial adhesion | Weak | Strong |
| Notched Izod impact | Variable, often low | Consistent, high |
| Phase domain size | Large and irregular | Fine and uniform |
| Lot-to-lot consistency | Poor | Good |
| Surface finish | Prone to flow marks | Uniform |
| Cost | Lower | Slightly higher |
Practical implication: when you compare two “PC/ABS” quotes, you are not comparing the same material unless both specify the ratio and the compatibilizer system. This is why the cheapest quote is so often the one that fails the drop test.
2. Property Profile
Typical values for a general-purpose, medium-PC-content (≈60:40) unfilled alloy. Always confirm against the specific grade TDS.
| Property | Typical Value | Unit | Test Standard |
| Density | 1.10–1.16 | g/cm³ | ISO 1183 |
| Melt flow rate (260 °C / 5 kg) | 8–25 | g/10 min | ISO 1133 |
| Tensile strength at yield | 50–62 | MPa | ISO 527 |
| Tensile modulus | 2,100–2,500 | MPa | ISO 527 |
| Flexural modulus | 2,200–2,600 | MPa | ISO 178 |
| Notched Izod impact (23 °C) | 400–800 | J/m | ISO 180 |
| Notched Izod impact (−30 °C) | 100–250 | J/m | ISO 180 |
| Charpy notched impact (23 °C) | 25–50 | kJ/m² | ISO 179 |
| HDT at 1.82 MPa | 100–125 | °C | ISO 75-2 |
| HDT at 0.45 MPa | 110–135 | °C | ISO 75-2 |
| Vicat softening point | 110–130 | °C | ISO 306 |
| Rockwell hardness | R105–R120 | — | ISO 2039-2 |
| Shrinkage (flow) | 0.4–0.7 | % | ISO 2577 |
| Water absorption (24 h) | 0.2–0.4 | % | ISO 62 |
| Dielectric strength | 15–25 | kV/mm | IEC 60243 |
| CTI | 250–600 | V | IEC 60112 |
| Flammability (FR grades) | UL94 V-0 @ 1.5 mm | — | UL94 / IEC 60695 |
What the Numbers Mean
- Notched Izod 400–800 J/m is about 2–3× general-purpose ABS and 60–90% of PC. It is the “survives a drop test” range.
- HDT 100–125 °C clears automotive interior temperatures (dashboards reach 90–110 °C in direct sun) and most electronics operating conditions, but not under-hood or reflow soldering.
- Shrinkage 0.4–0.7%, near-isotropic is why the alloy suits large parts with tight tolerances.
3. The PC:ABS Ratio Is the Master Variable
| Property | 40:60 | 60:40 | 70:30 |
| Notched Izod 23 °C (J/m) | 300–450 | 500–700 | 650–800 |
| HDT @1.82 MPa (°C) | 95–105 | 105–118 | 112–125 |
| Melt flow (260/5) | 20–30 | 10–20 | 8–15 |
| Density (g/cm³) | 1.10–1.12 | 1.13–1.15 | 1.14–1.16 |
| Relative cost | Low | Medium | High |
| Processability | Excellent | Good | Fair |
Commercial grades span 40:60 to 80:20, with 60:40 the most common. For a full treatment of how ratio drives properties, see our PC/ABS ratio guide.
4. Applications
PC/ABS’s application list is essentially a list of parts that must be both durable and presentable. The material’s combination of impact, heat resistance, dimensional stability, and surface finish maps onto a recognizable set of product categories, and within each category the specific grade family follows from the environment the part will see.
When reading the sections below, note that the grade selection is driven by the environment, not the product category. An electronics housing that sits indoors and one that sits outdoors in a charging station are both “electronics housings,” but the first uses general-purpose PC/ABS and the second needs either UV-stabilized PC/ABS or a switch to PC/ASA. Always read the application and the environment together.
4.1 Consumer Electronics and Business Machines
Laptop and monitor housings, printer chassis, copier panels, router enclosures, TV bezels. Thin-wall flow plus drop-test impact plus a paintable, Class-A surface — no other material covers all three at this price. Flame-retardant (UL94 V-0) grades dominate this segment because of internal power supplies and battery proximity.
4.2 Automotive Interior and Exterior Trim
Instrument panel carriers, A/B/C-pillar trim, door panels, center consoles, grille surrounds, mirror housings. Low-odor and low-VOC grades are mandatory for interior parts — standard PC/ABS emits styrene and other volatiles that fail OEM cabin-air requirements. Exterior parts exposed to sunlight require UV stabilization or PC/ASA.
4.3 EV Charging and Electrical Housings
Charging station enclosures, connector housings, meter boxes, breaker components. The drivers are flame retardancy (UL94 V-0), glow-wire resistance (IEC 60695-2), tracking resistance (CTI), and outdoor durability. Many outdoor charging housings are migrating to PC/ASA because PC/ABS yellows and embrittles under UV without heavy stabilization.
4.4 Medical and Healthcare Equipment
Diagnostic equipment housings, drug delivery device bodies, monitor bezels. Medical grades tolerate alcohols and quaternary ammonium disinfectants and, in some cases, gamma or EtO sterilization. PC/ABS is generally not suitable for autoclave sterilization at 121 °C+ — steam cycling stress-cracks it. For autoclavable transparent parts, consider PEI or PPSU.
4.5 Power Tools and Appliances
Tool housings, vacuum cleaner bodies, appliance control panels, coffee machine housings. Impact, heat, and paintability are what tool OEMs specify.
4.6 Industrial and Safety Equipment
Machine housings, control box covers, cable connectors, safety helmet shells (opaque grades). Where a part must absorb impact without shattering, PC/ABS is a strong candidate at a lower cost than glass-filled PC.
4.7 Application-to-Grade Map
| Application | Environment | Recommended Grade Family |
| Laptop / monitor housing | Indoor, drop-tested | High-flow PC/ABS, 60–65% PC |
| Printer / copier chassis | Indoor, FR required | FR PC/ABS, UL94 V-0 |
| Automotive instrument panel carrier | Interior, hot, low-VOC | Low-odor PC/ABS, 55–65% PC |
| Automotive exterior trim | Outdoor, UV | PC/ASA (not PC/ABS) |
| EV charger outdoor housing | Outdoor, FR, UV | FR PC/ASA or UV-stabilized FR PC/ABS |
| EV charger indoor housing | Indoor, FR | FR PC/ABS, UL94 V-0 |
| Medical diagnostic housing | Indoor, disinfectant exposure | Medical-grade PC/ABS |
| Power tool housing | Indoor/outdoor, impact | Impact-modified PC/ABS, 60–70% PC |
| Appliance control panel | Indoor, warm | General-purpose PC/ABS |
| Structural bracket | Indoor, load | GF10–GF30 PC/ABS |
| Snap-fit enclosure | Indoor | PC/ABS with ≥1.5% strain allowance |
4.8 Failure Modes to Anticipate
Three failure modes account for the majority of PC/ABS field failures, and all three are predictable at the design stage.
Environmental stress cracking (ESC). The combination of molded-in residual stress and contact with a chemical — solvent, mold release, adhesive, cleaner, or even hand cream — produces cracks that appear days to months after assembly. Mitigate by annealing parts that will contact chemicals and by qualifying every chemical that touches the part.
UV embrittlement. Outdoor exposure degrades the butadiene phase, and the part becomes brittle before it visibly yellows. Any part with a design life beyond one year outdoors should be specified as PC/ASA or with a qualified UV-stabilized grade and a documented weathering test (ISO 4892-2).
Creep under sustained load. PC/ABS creeps under continuous load, especially above 60 °C. A boss or snap fit sized for room-temperature yield strength can relax or crack in a warm environment. Size load-bearing features using creep data at the service temperature, not short-term tensile data.
5. Injection Molding
PC/ABS processes more easily than PC but far less forgiving than ABS. Moisture and cold molds are the two dominant causes of defects.
The processing behavior follows directly from the two-phase structure. The PC phase sets the viscosity and the drying requirement; the ABS phase sets the upper temperature limit and the flow character. Because both constraints must be satisfied simultaneously, the usable process window is narrower than for either base polymer — which is why the parameter table below is worth following closely rather than treating as a starting suggestion.
5.1 Drying
| Parameter | Recommendation |
| Drying temperature | 90–110 °C |
| Drying time | 3–4 hours (desiccant dryer) |
| Target moisture | ≤0.02% (200 ppm) |
| Dew point | ≤ −20 °C |
| Storage after drying | Sealed hopper, ≤8 hours |
Warning: do not exceed 120 °C drying. Over-drying degrades the ABS phase, producing a sticky hopper and yellowed parts.
5.2 Temperature and Pressure
| Parameter | Range |
| Melt temperature | 240–275 °C |
| Mold temperature | 60–90 °C (run hot for cosmetic parts) |
| Injection pressure | 80–140 MPa |
| Holding pressure | 40–70% of injection pressure |
| Back pressure | 0.3–1.0 MPa |
| Screw speed | Moderate (50–100 rpm) |
5.3 Mold Design Notes
| Feature | Recommendation |
| Nominal wall | 1.5–3.5 mm |
| Rib thickness | ≤60% of nominal wall |
| Gate | Hot runner or generous side gate; avoid pin-point on thick parts |
| Vent depth | 0.02–0.03 mm |
| Draft | 0.5–1° minimum; 1.5–2° textured |
| Shrinkage allowance | 0.4–0.7% |
5.4 Common Defects
| Defect | Likely Cause | Fix |
| Silver streaks / splay | Moisture | Re-dry to ≤0.02% |
| Weld line weakness | Low mold temperature, poor venting | Raise mold to 80–90 °C; add vents |
| Warpage | Uneven cooling, over-packing | Balance cooling; reduce hold pressure |
| Sink marks | Insufficient packing | Increase hold time; thin ribs |
| Yellowing | Melt too hot, long residence | Lower melt temp; reduce screw speed |
| Stress cracking | Residual stress + chemical | Anneal 80–90 °C 2–4 h; remove chemical |
6. PC/ABS Alloy vs Competing Materials
No material is chosen in isolation — it is always chosen against the alternatives on the same drawing. The comparison below places PC/ABS against the five materials it most often competes with, and states the single condition under which each alternative wins.
The pattern worth noting is that PC/ABS rarely wins on any single property outright. It is not the toughest (PC is), not the cheapest (ABS and HIPS are), not the most chemically resistant (PC/PBT is), and not the most weather-stable (PC/ASA is). It wins on the balance — and in enclosure applications, balance is usually what the requirement list actually asks for. A design that specifies “structural, drop-tested, warm, paintable, affordable” is describing PC/ABS, even if it never names it.
6.1 PC/ABS vs ABS
ABS is cheaper and flows better, but PC/ABS has 2–4× the impact strength and 20–40 °C more heat resistance. Choose ABS for cost-driven parts under 80 °C; PC/ABS for anything dropped or heated.
6.2 PC/ABS vs PC
Pure PC is tougher, more heat-resistant, and transparent. PC/ABS flows better, costs less, and is less notch-sensitive. Choose PC for optical or extreme-heat parts; PC/ABS for opaque structural enclosures.
6.3 PC/ABS vs PC/PBT
PC/PBT resists fuels, oils, and many solvents that destroy PC/ABS and has better low-temperature impact. PC/ABS is cheaper and easier to process. Choose PC/PBT for automotive exterior parts exposed to fuel or road chemicals.
6.4 PC/ABS vs PC/ASA
PC/ASA is formulated for outdoor weathering and retains color and impact under UV and humidity far better than PC/ABS. For any part in direct sunlight, PC/ASA is usually the better choice despite the price.
6.5 PC/ABS vs HIPS
High-impact polystyrene (HIPS) is much cheaper but has one-third the impact strength and half the heat resistance. HIPS suits low-cost, low-demand enclosures; PC/ABS is for anything structural or warm.
6.6 Comparison Summary
| Material | Notched Izod 23 °C (J/m) | HDT @1.82 MPa (°C) | Density (g/cm³) | Relative Cost | Best For |
| ABS | 150–350 | 80–95 | 1.04–1.07 | $ | Cost-driven, plating |
| HIPS | 60–150 | 70–85 | 1.04–1.06 | $ | Low-cost enclosures |
| PC/ABS | 400–800 | 100–125 | 1.10–1.16 | $$ | Structural enclosures |
| PC/PBT | 500–900 | 110–130 | 1.20–1.30 | $$$ | Chemical / fuel exposure |
| PC/ASA | 450–700 | 100–120 | 1.12–1.18 | $$$ | Outdoor / UV |
| PC | 600–900 | 128–138 | 1.19–1.22 | $$$ | Optical, extreme heat |
7. Selecting and Substituting a Grade
| Requirement | Grade to Specify |
| General enclosure | Standard PC/ABS, MFR 10–15, PC ≥55% |
| Thin-wall / long flow | High-flow PC/ABS, MFR 18–30 |
| Flame retardant | FR PC/ABS, UL94 V-0 at your wall thickness |
| Automotive interior | Low-odor / low-VOC PC/ABS |
| Outdoor / UV | Switch to PC/ASA or UV-stabilized PC/ABS |
| Stiffness + low warp | GF10–GF30 PC/ABS |
| Cold drop test | ≥65% PC with low-temp impact modifier |
| Plating | Plating-grade ABS (not standard PC/ABS) |
Ordering checklist: request (1) TDS with ratio or DSC trace, (2) COA for the specific lot, (3) UL yellow card if FR is claimed, and (4) a sample for your own drop and heat testing. For FR grades, confirm V-0 at your wall thickness — a 3.0 mm rating does not transfer to 1.2 mm.
Equivalent substitution typically takes three to six weeks: define acceptance criteria (not the incumbent grade number), screen candidates on paper, run a mold trial for shrinkage and warp, test to standard (drop, heat aging, chemical, flammability on the finished part), run pilot lots for consistency, then freeze the specification.
8. Grade Families and What They Contain
The PC:ABS ratio sets the baseline, but the grade family determines what the material is actually formulated to do. These are the families you will encounter when specifying.
| Grade Family | Typical Formulation | Key Property Boost | Typical Applications |
| General purpose | 55–60% PC, standard compatibilizer | Balanced | Electronics housings, appliances |
| High flow | 50–60% PC, flow modifier | MFR 18–30 g/10 min | Thin-wall, long-flow parts |
| Flame retardant | FR package (phosphorus or brominated) | UL94 V-0 at 1.5 mm | IT/EE equipment, EV housings |
| Low-odor / low-VOC | Purified ABS phase, devolatilization | VOC < 30 µgC/g | Automotive interior |
| UV-stabilized | HALS + UVA package | Slowed yellowing | Semi-outdoor parts |
| Glass-filled | GF10–GF30 | Stiffness, low warpage | Structural brackets |
| Impact-modified | MBS or acrylic modifier | Low-temperature impact | Cold drop tests |
| Plating-grade | High-butadiene ABS phase | Plateable surface | Decorative parts |
| Medical grade | USP Class VI / ISO 10993 compliant | Biocompatibility | Diagnostic equipment |
Choosing a family. Start with the general-purpose family and add only what your application demands. Each added package — FR, UV, glass — consumes part of the property budget, and a heavily loaded grade can underperform a simpler one on impact. The right question is never “what is the best PC/ABS?” but “which family does my requirement list actually need?”
8.1 Glass-Filled PC/ABS
GF10–GF30 grades raise stiffness substantially but reduce impact strength and elongation. They also introduce anisotropic shrinkage (flow direction versus cross-flow), which must be accounted for in tool design.
| Property | Unfilled PC/ABS | GF10 | GF20 | GF30 |
| Flexural modulus (MPa) | 2,200–2,600 | 3,200–3,800 | 4,500–5,500 | 6,000–7,000 |
| Notched Izod 23 °C (J/m) | 400–800 | 120–200 | 90–150 | 70–120 |
| Shrinkage, flow (%) | 0.4–0.6 | 0.3–0.5 | 0.2–0.4 | 0.1–0.3 |
| Shrinkage, cross-flow (%) | 0.4–0.6 | 0.4–0.6 | 0.5–0.8 | 0.6–0.9 |
Note the growing gap between flow and cross-flow shrinkage as glass content rises. This differential is the reason glass-filled grades warp if gating is not designed for it — gate at the thick end and expect more shrinkage across the flow.
9. Incoming Inspection: What to Check on Every Lot
A supplier’s TDS describes the material they intend to ship. Incoming inspection confirms the material they actually shipped. For PC/ABS, four checks catch the overwhelming majority of out-of-spec lots, and all four are fast and inexpensive.
| Check | Method | Frequency | What It Catches |
| Density | ISO 1183 | Every lot | Ratio drift, filler substitution |
| Melt flow rate | ISO 1133 | Every lot | Molecular weight change, regrind loading |
| Notched Izod | ISO 180 | Per lot or per batch | Impact modifier missing or degraded |
| DSC (PC Tg) | ISO 11357-2 | Per batch | Ratio verification |
The most valuable of these is density, because it is fast, needs no special specimen preparation, and detects the most common supplier failure — quietly shifting the ratio downward to save cost. For a 60:40 grade, a density more than 0.02 g/cm³ below the specification is a strong signal that the PC content has dropped.
Melt flow rate catches a different problem: excess regrind or thermal degradation during compounding. A lot that meets density but runs 30% high on MFR has likely been over-processed, and its impact strength will be lower than the TDS claims.
Keep a retained sample of every approved lot. When a field failure occurs, having the original reference material on hand is the difference between diagnosing the cause in a week and arguing about it for months.
10. Frequently Asked Questions
Is PC/ABS alloy the same as PC/ABS blend?
Practically yes. Both refer to the polycarbonate–ABS two-phase material. “Alloy” often implies a compatibilized blend, but the terms are used interchangeably.
What is the best PC:ABS ratio?
There is no universal best. 60:40 is the most common commercial ratio. The right ratio is the lowest PC content that meets your impact and heat requirements — higher PC raises cost and reduces flow.
Is PC/ABS food safe?
Not inherently. Food-contact grades meeting FDA 21 CFR and EU 10/2011 exist, but you must specify one and verify with a migration test. Standard industrial grades are not for food contact.
Can PC/ABS be recycled?
Yes — mechanically. rPC/ABS grades are increasingly available, but sorting mixed PC/ABS streams is difficult and recycled impact strength is often reduced. Qualify the actual recycled content before specifying.
Why does my PC/ABS part crack in the field?
Almost always environmental stress cracking: molded-in residual stress plus contact with a solvent, mold release, adhesive, or cleaner. Anneal the part and eliminate the chemical.
Does PC/ABS yellow outdoors?
Yes. The butadiene phase degrades under UV. UV-stabilized grades slow it, but for long-term outdoor exposure, PC/ASA is the correct material.
What is the melting point of PC/ABS?
There is none — both components are amorphous. The ABS phase softens near 100 °C and the PC phase has a glass transition near 145–150 °C (measurable by DSC to ISO 11357-2). Design with HDT and Vicat, not “melting point.”
How do I know if a PC/ABS grade contains glass fiber?
Check the density — glass raises density above ~1.18 g/cm³ — and ask for the ash content. TGA to ISO 11358 will quantify the filler. A glass-filled grade also shows noticeably lower elongation in a tensile test to ISO 527.
What is the difference between general-purpose and high-flow PC/ABS?
High-flow grades add a flow modifier that raises MFR to 18–30 g/10 min at the cost of some impact strength and heat resistance. Use them only when thin-wall filling or long flow length demands it.
Is there a PC/ABS grade for food contact?
Yes, but you must specify it explicitly. Food-contact grades meet FDA 21 CFR 177.1020 / 177.1040 and EU 10/2011, and require migration testing. Standard industrial grades must never be used for food contact.
How long does it take to qualify an equivalent PC/ABS grade?
Typically three to six weeks: define acceptance criteria, screen candidates on paper, run a mold trial for shrinkage and warp, test to standard (drop, heat aging, chemical resistance, flammability on the finished part), run pilot lots for consistency, then freeze the specification.
What is the difference between a “generic” and a “branded” PC/ABS?
Branded grades come from major producers with documented ratios, UL yellow cards, and OEM approvals. Generic compounds are made by smaller compounders and vary widely in consistency. A well-controlled generic can be an excellent value; an uncontrolled one is a hidden cost. The test is documentation — if the supplier will state the ratio and provide a COA, the material can be evaluated on its merits.
11. Next Steps
PC/ABS alloy selection comes down to three decisions: how much PC you need (ratio), what flame and regulatory rating is required, and what environment the part will see (interior vs outdoor, chemical exposure). Get those three on paper and the grade follows.
We supply PC/ABS alloy across the full ratio range, including general-purpose, high-flow, flame-retardant (UL94 V-0), low-odor automotive, glass-filled, and custom-compatibilized grades from our own compounding facility. Because we compound in-house, we can tune the ratio, the compatibilizer, and the impact modifier system to your exact drop, heat, and surface requirements, and run a sample batch before you commit to production tonnage.
What we can send you:
- Full TDS with ratio and DSC verification
- COA and batch traceability
- UL yellow card copies for FR grades
- Free samples for your own testing
[Ask for an Equivalent Grade Quote →]
Related Reading
- PC/ABS Blend: The Complete Guide to Properties, Grades and Applications
- PC/ABS vs ABS vs PC: Which One for Your Enclosure?
- PC/ABS Ratio Explained: How the PC:ABS Blend Ratio Changes Performance
- PC/ABS Processing Guide: Drying, Melt Temperature and Mold Design
- PC/PBT Alloy: Properties, Chemical Resistance and Applications
- Flame-Retardant PC/ABS: UL94 V-0 Grades for IT and EV Housings