PC/ABS is a polycarbonate–acrylonitrile butadiene styrene alloy that balances PC’s strength and heat resistance against ABS’s processability and cost.
If you need a part with better impact strength and heat resistance than ABS, but tighter tolerances and lower cost than pure PC, PC/ABS resin is almost always the right answer. The single biggest variable is the PC:ABS ratio — everything from your part’s stiffness to its chemical resistance and surface finish traces back to that number.
What Is PC/ABS?
PC/ABS is a thermoplastic alloy — a physical blend of polycarbonate (PC) and acrylonitrile butadiene styrene (ABS). It is not a copolymer and it is not a compound in the filled sense; it is a two-phase polymer blend in which ABS is dispersed within a continuous PC matrix (or vice versa, depending on the ratio).
The reason the alloy exists at all comes down to complementary weaknesses:
| Material | Strength | Weakness |
| PC (polycarbonate) | Very high impact strength, high heat resistance (HDT ~130–135 °C), excellent dimensional stability | High melt viscosity, notch-sensitive, poor chemical resistance, expensive, difficult to mold thin walls |
| ABS | Excellent processability, good surface finish, low cost, easy to color and plate | Moderate heat resistance (HDT ~80–95 °C), lower impact strength |
| PC/ABS alloy | Takes the best of both: impact strength and heat resistance from PC, flow and finish from ABS | Still notched-sensitive, still limited chemical resistance |
By blending the two, you get a material with a heat deflection temperature typically between 100 °C and 125 °C, notched Izod impact strength in the range of 400–800 J/m, and a melt flow rate that is far more forgiving than unmodified PC.
Why the Alloy Matters Commercially
PC/ABS is the default material for large, thin-walled, aesthetically demanding enclosures — laptop housings, automotive interior trim, EV charging station covers, power tool bodies, medical device housings. Those applications share three requirements that neither PC nor ABS satisfies alone: they need to survive a drop test (impact), they need to survive a hot dashboard or a warm electronics bay (heat), and they need to come out of the mold with a flawless Class-A surface (flow and finish).
2. The PC:ABS Ratio — Why It Is the Only Number That Matters
If you take one thing from this guide, take this: the PC:ABS ratio is the primary design variable in PC/ABS. Most commercial grades fall between 40:60 and 80:20. Here is how the ratio changes the material:
| Property | Lower PC (e.g. 40:60) | Higher PC (e.g. 70:30) |
| Notched Izod impact | ~300–450 J/m | ~600–800 J/m |
| Heat deflection temperature (1.82 MPa) | ~95–105 °C | ~110–125 °C |
| Melt flow rate | Higher (easier to mold thin walls) | Lower (stiffer melt, harder to fill) |
| Density | ~1.10 g/cm³ | ~1.15 g/cm³ |
| Cost | Lower | Higher |
| Surface finish | Good | Requires careful mold temperature control |
| Chemical resistance | Slightly better (more ABS) | Worse (more PC, more stress-cracking risk) |
| UV / weathering | Poor without ASA or additives | Poor without ASA or additives |
Practical rule of thumb: For a thin-wall electronics enclosure that must pass a 1 m drop test at −20 °C, specify ≥60% PC. For a large cosmetic part where flow length and cost dominate, 45–55% PC is usually sufficient.
How to verify the ratio you are actually buying: Ask your supplier for a differential scanning calorimetry (DSC) trace. The PC glass transition temperature (Tg ≈ 145–150 °C) appears as a distinct inflection. Comparing the magnitude of that signal against a known reference is the standard way to ballpark the PC content. Suppliers who cannot produce a DSC trace are almost certainly selling you an inconsistent blend.
3. Key Properties and Typical Data
The following table represents typical values for a general-purpose, medium-PC-content PC/ABS grade. Always confirm against the specific grade’s TDS — values vary significantly by supplier and ratio.
| Property | Typical Value | Unit | Test Standard |
| Density | 1.10–1.16 | g/cm³ | ISO 1183 |
| Melt flow rate (260 °C / 5 kg) | 8–25 | g/10 min | ISO 1133 |
| Tensile strength at yield | 50–62 | MPa | ISO 527 |
| Tensile modulus | 2,100–2,500 | MPa | ISO 527 |
| Flexural modulus | 2,200–2,600 | MPa | ISO 178 |
| Notched Izod impact (23 °C) | 400–800 | J/m | ISO 180 |
| Notched Izod impact (−30 °C) | 100–250 | J/m | ISO 180 |
| Charpy notched impact (23 °C) | 25–50 | kJ/m² | ISO 179 |
| HDT at 1.82 MPa | 100–125 | °C | ISO 75-2 |
| HDT at 0.45 MPa | 110–135 | °C | ISO 75-2 |
| Vicat softening point | 110–130 | °C | ISO 306 |
| Rockwell hardness | R105–R120 | — | ISO 2039-2 |
| Shrinkage (flow direction) | 0.4–0.7 | % | ISO 2577 |
| Water absorption (24 h) | 0.2–0.4 | % | ISO 62 |
| Dielectric strength | 15–25 | kV/mm | IEC 60243 |
What the Numbers Mean in Practice
- HDT of 100–125 °C means the part holds its shape through automotive interior temperatures (dashboard surfaces can reach 90–110 °C in direct sun) and through most electronics operating conditions, but it will not survive under-hood or reflow-soldering environments. Those need PBT, PA, or PPS.
- Notched Izod of 400–800 J/m is roughly 2–4× that of general-purpose ABS and around 40–60% of pure PC. It is the “enough for a drop test” range for handheld and portable products.
- Shrinkage of 0.4–0.7% is low and fairly isotropic compared to semi-crystalline resins, which is why PC/ABS is favored for parts with tight dimensional tolerances across a large footprint.
4. Applications: Where PC/ABS Earns Its Place
4.1 Consumer Electronics and Business Machines
Laptop and monitor housings, printer chassis, copier panels, router enclosures. The combination of thin-wall flow, drop-test impact, and the ability to take a perfect paint or texture makes PC/ABS the incumbent. Flame-retardant grades (UL94 V-0) dominate this segment because of internal power supplies and battery proximity.
4.2 Automotive Interior and Exterior Trim
Instrument panel carriers, A/B/C-pillar trim, door panels, center consoles, grille surrounds, mirror housings. Low-odor and low-VOC (volatile organic compound) grades are mandatory for interior parts — standard PC/ABS can emit styrene and other volatiles that fail OEM cabin-air requirements. For exterior parts that see direct sunlight, PC/ABS must be UV-stabilized or replaced with PC/ASA.
4.3 EV Charging and Electrical Housings
EV charging station enclosures, connector housings, meter boxes, breaker components. Here the drivers are flame retardancy (UL94 V-0), glow-wire resistance (IEC 60695-2), tracking resistance (CTI), and outdoor durability. Many outdoor charging housings are migrating from PC/ABS to PC/ASA specifically because PC/ABS yellows and embrittles under UV without heavy stabilization.
4.4 Medical and Healthcare Equipment
Diagnostic equipment housings, drug delivery device bodies, monitor bezels. Medical-grade PC/ABS must tolerate common disinfectants (alcohols, quaternary ammonium compounds) and, for some grades, gamma or EtO sterilization. Note that PC/ABS is generally not suitable for autoclave sterilization at 121 °C+ — steam cycling will stress-crack it. For autoclavable transparent parts, consider PEI or PPSU instead.
4.5 Power Tools and Appliances
Tool housings, vacuum cleaner bodies, appliance control panels, coffee machine housings. The blend of impact resistance, heat resistance, and paintable surface is what tool OEMs specify.
5. Processing PC/ABS: Injection Molding Guide
PC/ABS processes much more easily than pure PC, but it is far less forgiving than ABS. Moisture and over-drying are the two most common causes of defects.
5.1 Drying (Non-Negotiable)
PC absorbs atmospheric moisture and hydrolyzes at melt temperature — this shows up as silver streaks, splay, and a permanent loss of impact strength. PC/ABS must be dried before every run.
| Parameter | Recommendation |
| Drying temperature | 90–110 °C |
| Drying time | 3–4 hours (desiccant dryer) |
| Target moisture content | ≤ 0.02% (200 ppm) |
| Dryer type | Desiccant (hot-air ovens are not sufficient) |
| Storage after drying | Sealed hopper, ≤ 8 hours |
Warning: Do not exceed 120 °C drying temperature. Over-drying causes the ABS phase to degrade and can create a sticky, blocked hopper and a yellowed part.
5.2 Melt and Mold Temperature
| Parameter | Range |
| Melt temperature | 240–275 °C |
| Mold temperature | 60–90 °C |
| Injection pressure | 80–140 MPa |
| Holding pressure | 40–70% of injection pressure |
| Back pressure | 0.3–1.0 MPa |
| Screw speed | Moderate (50–100 rpm) |
Mold temperature matters more than most operators expect. A mold running at 60 °C will produce a dull, weld-line-prone part with high molded-in stress; the same material at 80–90 °C produces a glossy Class-A surface with better impact retention. For cosmetic parts, always run the hot side of the window.
5.3 Common Defects and Fixes
| Defect | Likely Cause | Fix |
| Silver streaks / splay | Moisture | Re-dry to ≤0.02%; check dryer dew point |
| Weld line weakness | Low mold temperature, poor venting | Raise mold temp to 80–90 °C; add vents at weld locations |
| Warpage | Uneven cooling, high packing | Balance cooling circuits; reduce hold pressure; check gate location |
| Sink marks | Insufficient packing, thick ribs | Increase hold time; reduce rib thickness to ≤60% of wall |
| Short shots | Low melt temp, low injection speed | Raise melt to 260–270 °C; increase injection speed |
| Yellowing / burning | Melt temperature too high, long residence time | Lower melt temp; reduce screw speed; check for dead spots |
| Stress cracking in service | Residual stress + chemical contact | Anneal at 80–90 °C for 2–4 h; avoid incompatible mold releases |
5.4 Secondary Operations
- Painting and printing: PC/ABS takes paint, pad printing, and laser marking well. Always test the solvent carrier — aggressive solvents cause stress cracking.
- Electroplating: Standard PC/ABS is generally not plating-grade (ABS is). Plating a PC/ABS part requires a specially formulated grade with higher butadiene content.
- Ultrasonic welding: Works well; PC/ABS is compatible with itself and with ABS. Not compatible with PC or PMMA without an energy director design change.
- Laser welding: Some grades are laser-transparent/laser-absorbing pairs for through-welding.
5.5 Annealing: The Most Underused Fix
Molded-in residual stress is the root cause of most in-service PC/ABS failures, and annealing is the cheapest way to eliminate it. A properly annealed part can see its environmental stress cracking (ESC) resistance improve by a factor of two to three.
| Parameter | Recommendation |
| Annealing temperature | 80–90 °C (below HDT, above service temperature) |
| Annealing time | 2–4 hours, depending on wall thickness |
| Atmosphere | Air-circulating oven; support the part to prevent sag |
| Cooling | Slow, in the oven, to avoid re-introducing stress |
| When to anneal | Any part that will contact solvents, adhesives, or cleaners; any part with high molded-in stress (long flow, tight gates) |
Do not anneal a part that has already been painted or assembled — the temperature will damage coatings and distort snap fits. Anneal before secondary operations.
5.6 Regrind and Recycled Content
PC/ABS tolerates regrind reasonably well at low percentages, but impact strength drops faster than any other property. A practical guideline:
| Regrind Level | Effect on Notched Izod | Recommendation |
| 0% (virgin) | Baseline | Cosmetic parts, structural parts, safety-critical |
| 10–15% | −5 to −10% | Acceptable for most non-cosmetic parts |
| 15–25% | −15 to −30% | Only with re-stabilization and impact modifier top-up |
| >25% | −30%+ and inconsistent | Not recommended without full requalification |
Always dry regrind as carefully as virgin material, and always blend regrind uniformly — inconsistent blending is the number-one cause of lot-to-lot property variation in recycled PC/ABS.
6. PC/ABS vs Competing Materials
6.1 PC/ABS vs ABS
ABS is cheaper, lighter (1.04–1.07 g/cm³), flows better, and plates more easily. PC/ABS wins on impact strength (2–4×), heat resistance (HDT +20 to +40 °C), and dimensional stability. Choose ABS when the part is cost-driven, needs electroplating, and never sees more than ~80 °C. Choose PC/ABS when the part must survive a drop test, sit near heat, or hold tight tolerances over a large area.
6.2 PC/ABS vs PC
Pure PC has higher impact strength (notched Izod often 600–900 J/m), higher HDT (~130–135 °C), and better optical clarity when unfilled. PC/ABS wins on flow (fills thin walls at lower pressure), cost, and colorability, and it is less notch-sensitive. Choose PC for transparent parts, optical components, and maximum heat + impact. Choose PC/ABS for opaque structural enclosures where processability and cost matter.
6.3 PC/ABS vs PC/PBT
PC/PBT is the chemical-resistance champion — it resists fuels, oils, and many solvents that would destroy PC/ABS. PC/PBT also has better low-temperature impact. PC/ABS is cheaper and easier to process. Choose PC/PBT for automotive exterior parts exposed to fuel, grease, or road chemicals. Choose PC/ABS for interiors and electronics where chemical exposure is limited.
6.4 PC/ABS vs PC/ASA
PC/ASA is formulated for outdoor weathering. It retains color and impact under UV and humidity far better than PC/ABS. If your part sees direct sunlight, PC/ASA is almost always the better choice despite the higher price. See our dedicated PC/ASA guide for weathering data.
7. Selecting the Right PC/ABS Grade
| Requirement | Grade to Specify |
| General-purpose enclosure | Standard PC/ABS, MFR 10–15, PC ≥55% |
| Thin-wall / long flow | High-flow PC/ABS, MFR 18–30 |
| Flame retardant (IT/EE) | FR PC/ABS, UL94 V-0 at 1.5 mm |
| Automotive interior | Low-odor / low-VOC PC/ABS |
| Outdoor / UV exposure | Switch to PC/ASA or specify UV-stabilized PC/ABS |
| Glass reinforcement | GF10–GF30 PC/ABS for stiffness and low warpage |
| High impact at low temp | High-PC-content PC/ABS (≥65%) with impact modifier |
| Plating | Plating-grade ABS (not standard PC/ABS) |
Ordering checklist: Always request (1) the TDS with the PC:ABS ratio or DSC trace, (2) a COA for the specific lot, (3) UL yellow card if flame retardancy is claimed, and (4) a sample for your own drop/heat testing. For FR grades, confirm the V-0 rating at your wall thickness — a 3.0 mm V-0 rating does not transfer to a 1.2 mm wall.
7.1 Branded vs Generic PC/ABS
The PC/ABS market splits into branded grades from the major producers and generic/unbranded compounds. The difference is real but narrower than the price gap suggests.
| Factor | Branded (Covestro, SABIC, Chi Mei, LG, Trinseo) | Generic / Unbranded |
| Lot-to-lot consistency | Very high | Variable |
| Documented PC:ABS ratio | Usually yes | Often unavailable |
| UL yellow card | Available | Frequently absent or unverifiable |
| Automotive OEM approvals | Yes | No |
| Price | Baseline + 10–30% | Baseline |
| Lead time | Longer for specialty grades | Shorter, more flexible |
| Support | Technical service, failure analysis | Limited |
Our position: we supply both. For automotive interior, medical, and any part with a UL requirement, use a branded grade. For general industrial enclosures where the part is not safety-critical and you have validated the sample yourself, a well-controlled generic compound is a legitimate cost-reduction path — provided your supplier can document the ratio and provide a COA.
7.2 Equivalent Grade Substitution
If a branded PC/ABS grade is unavailable, on allocation, or too expensive, an equivalent substitute can often be qualified in three to six weeks:
- Establish the requirement, not the grade. Write down the actual acceptance criteria: notched Izod at −20 °C, HDT at 1.82 MPa, MFR range, FR rating at your wall thickness, color, and finish. Do not simply copy the incumbent grade number.
- Screen candidates on paper. Compare TDS values against your criteria. Eliminate anything that misses a hard requirement (FR rating, HDT) regardless of price.
- Run a mold trial. Process the candidate on the same tool with the same parameters. Measure shrinkage and warp against the incumbent — dimensional mismatch is the most common reason a substitution fails.
- Test to the standard. Drop test, heat aging, chemical exposure, and (for FR parts) re-verify the flammability rating on the finished part, not just the pellet.
- Run a pilot lot. Confirm lot-to-lot consistency over at least three production lots before switching fully.
- Document and lock. Freeze the specification and keep a retained sample of the incumbent for future comparison.
This qualification process is exactly what our compounding facility supports — we can supply trial quantities, adjust the formulation if a candidate misses a target, and scale to production tonnage once the grade is approved.
8. Frequently Asked Questions
Is PC/ABS the same as PC-ABS alloy?
Yes. “PC/ABS,” “PC-ABS,” and “PC/ABS alloy” all refer to the same polycarbonate–ABS blend. Some suppliers use “alloy” to imply a compatibilized blend, but the terms are interchangeable in practice.
Is PC/ABS food safe?
Not inherently. PC/ABS can be formulated to meet FDA 21 CFR and EU 10/2011 food-contact requirements, but you must specify a food-contact grade and verify with a migration test. Standard industrial grades should never be used for food contact.
Can PC/ABS be recycled?
Yes. PC/ABS is mechanically recyclable, and post-industrial and post-consumer recycled (rPC/ABS) grades are increasingly available. The main issue is sorting — separating PC/ABS from ABS and PC in a mixed stream is difficult, and recycled material often shows reduced impact strength. Specify rPC/ABS only after qualifying the actual recycled content and properties.
Does PC/ABS yellow over time?
Yes, under UV exposure. The butadiene phase in the ABS component is the primary degradation site. UV-stabilized grades slow this significantly, but for long-term outdoor exposure, PC/ASA is the correct answer.
What is the melting point of PC/ABS?
PC/ABS does not have a true melting point because both components are amorphous. It softens over a range: the ABS phase softens first (around 100 °C), and the PC phase has a glass transition around 145–150 °C. Use HDT and Vicat values (not “melting point”) for design.
Why does my PC/ABS part crack in service?
The overwhelming majority of in-service PC/ABS failures are environmental stress cracking (ESC): molded-in residual stress combined with contact with an incompatible chemical (solvent, mold release, adhesive, cleaner, or even hand cream). The fix is a two-part approach — anneal the part to relieve stress, and eliminate the offending chemical.
9. Next Steps
Choosing the right PC/ABS grade comes down to three decisions: how much PC do you actually need (ratio), what flame and regulatory rating must it meet, and what environment will the part see (interior vs outdoor, chemical exposure).
We supply PC/ABS in the full range of ratios and grades — general-purpose, high-flow, flame-retardant (UL94 V-0), low-odor automotive, glass-filled, and custom-formulated alloys from our own compounding facility. Because we compound in-house, we can tune the PC:ABS ratio and the additive package to your exact drop, heat, and surface requirements, and we can run a sample batch before you commit to production tonnage.
What we can send you:
- Full TDS with ratio and DSC verification
- COA and batch traceability for any lot
- UL yellow card copies for FR grades
- Free samples for your own testing
[Request TDS and Samples →] | [Ask for an Equivalent Grade Quote →]
Related Reading
- PC/ABS vs ABS vs PC: Which One for Your Enclosure?
- PC/ABS Ratio Explained: How the PC:ABS Blend Ratio Changes Performance
- Flame-Retardant PC/ABS: UL94 V-0 Grades for IT and EV Housings
- PC/ABS vs PC/ASA for Outdoor and UV-Exposed Parts
- PC/PBT Alloy: Properties, Chemical Resistance and Applications
- PC vs PMMA (Acrylic): Optical Clarity, Impact and Cost