PC/ABS is a two-phase alloy, and that changes the processing rules. The PC phase demands thorough drying and high temperatures; the ABS phase degrades if you over-dry or overheat. Finding the window between those two constraints is what separates a clean run from a scrap bin. This guide covers drying, temperature, mold design, and defect troubleshooting in the order you will encounter them.
One framing point before the details: with PC/ABS, almost every defect you will encounter traces back to one of three root causes — moisture in the melt, a mold that is too cold, or a barrel temperature that is too high for too long. Defect tables list dozens of symptoms, but they collapse into those three. If you are troubleshooting and unsure where to start, check the moisture content first, the mold temperature second, and the residence time third. That order resolves the majority of cases.
It also helps to understand why the material is sensitive to these three variables. The PC phase hydrolyzes on contact with water at melt temperature, cleaving polymer chains and permanently reducing molecular weight — this is irreversible and cannot be recovered by re-drying. The two-phase morphology needs time to develop, which requires a hot mold; a cold mold freezes in a poorly formed structure with weak phase boundaries. And the ABS phase has a thermal ceiling that, once exceeded, degrades into visible yellowing and odor. Respect those three constraints and PC/ABS is a well-behaved material.
1. Drying: The Non-Negotiable First Step
Polycarbonate hydrolyzes at melt temperature — the water molecule attacks the carbonate linkage and cleaves the polymer chain. The result is a permanent loss of molecular weight, which shows up as silver streaks, splay marks, and brittle parts that pass a visual inspection but fail in the field.
1.1 Drying Parameters
| Parameter | Recommendation | Notes |
| Drying temperature | 90–110 °C | 100 °C is a good starting point |
| Drying time | 3–4 hours | Longer for thick pellets or humid climates |
| Target moisture | ≤0.02% (200 ppm) | Verify with a moisture analyzer |
| Dryer type | Desiccant (dehumidifying) | Hot-air ovens are not sufficient |
| Dew point | ≤ −20 °C | Critical for achieving 200 ppm |
| Post-drying storage | Sealed hopper, ≤8 hours | Re-dry if exposed longer |
1.2 The Over-Drying Trap
There is a real upper bound: do not exceed 120 °C. Above that, the ABS phase begins to degrade, the pellets become sticky and bridge in the hopper, and the molded part yellows. Over-drying is a less common failure than under-drying, but it happens in plants that “crank up the heat to be safe.”
Field note: In humid climates, pellets can absorb moisture during conveying and storage even after drying. Keep the dried material in a sealed, desiccated hopper and minimize the path from dryer to machine. A 15-minute exposure to humid plant air can push a marginal lot back over the 200 ppm line.
2. Temperature Settings
2.1 Melt Temperature
| Zone | Typical Setting |
| Feed zone | 220–240 °C |
| Compression zone | 240–260 °C |
| Metering zone | 250–270 °C |
| Nozzle | 250–270 °C |
The recommended melt temperature window is 240–275 °C. Below 240 °C, the melt is too stiff to fill thin walls and you get short shots and high molded-in stress. Above 275 °C, the ABS phase begins to degrade and you get splay, odor, and yellowing.
2.2 Mold Temperature
| Requirement | Mold Temperature |
| Non-cosmetic structural part | 60–70 °C |
| General cosmetic part | 70–80 °C |
| Class-A surface / high gloss | 80–90 °C |
| Maximum impact retention | 80–90 °C |
Mold temperature is the most under-set parameter in PC/ABS molding. A mold running at 60 °C produces a dull part with weak weld lines and high residual stress, even though the part looks acceptable at first glance. Raising the mold to 80–90 °C produces a glossy surface, stronger weld lines, and better impact retention — because slower cooling gives the two polymer phases time to develop proper morphology.
2.3 Pressure and Speed
| Parameter | Range |
| Injection pressure | 80–140 MPa |
| Holding pressure | 40–70% of injection pressure |
| Back pressure | 0.3–1.0 MPa |
| Injection speed | Medium to fast for thin walls |
| Screw speed | Moderate (50–100 rpm) |
| Cushion | 3–8 mm |
Keep screw speed moderate. High screw speed generates shear heat that can locally exceed the degradation threshold, and PC/ABS is more shear-sensitive than ABS.
3. Mold Design for PC/ABS
PC/ABS’s high melt viscosity and low shrinkage make mold design slightly different from ABS. Use the material’s own test data as your design basis — density via ISO 1183, shrinkage via ISO 2577, and flow length via ISO 1133 melt flow rate — rather than carrying over ABS assumptions.
3.1 Wall Thickness
| Feature | Recommendation |
| Nominal wall | 1.5–3.5 mm |
| Minimum wall | 1.0 mm (with high-flow grade) |
| Maximum wall | 4.0 mm (above this, sink risk rises) |
| Rib thickness | ≤60% of nominal wall |
3.2 Gates
| Gate Type | Suitability | Notes |
| Direct / sprue | Good | Simple, but leaves a visible mark |
| Side gate | Good | Common for flat parts |
| Submarine gate | Fair | Automatically degrades; watch shear at gate |
| Hot runner | Excellent | Best for cosmetic parts and multi-cavity |
| Pin-point | Poor for thick parts | High shear, freeze-off risk |
Gate location matters more than gate type. Place gates so that flow front meets at a low-stress location (ideally a non-cosmetic area), and size the gate generously — undersized gates cause jetting, high shear, and stress-cracking at the gate. A gate that is too small is a leading cause of delayed cracking at the sprue.
3.3 Venting
PC/ABS generates volatiles (especially styrene from the ABS phase). Poor venting traps them and causes burn marks, splay, and short shots.
- Vent depth: 0.02–0.03 mm
- Vent width: 3–5 mm
- Vents at: end of fill, weld line locations, blind corners, and around inserts
3.4 Cooling and Draft
- Cooling channels should follow the part contour at uniform distance for even cooling (uneven cooling is the main cause of warpage).
- Draft angle: 0.5–1° minimum; 1.5–2° for textured surfaces.
- Ejector pins should be generously sized — PC/ABS at the cold end of the window is stiff, and small pins can crack the part on ejection.
3.5 Shrinkage Allowance
Typical shrinkage for PC/ABS is 0.4–0.7%, and it is fairly isotropic compared to semi-crystalline resins. However, shrinkage varies with PC content and wall thickness:
| PC Content | Shrinkage (flow) | Shrinkage (cross-flow) |
| 40% | 0.5–0.7% | 0.5–0.7% |
| 60% | 0.4–0.6% | 0.4–0.6% |
| 80% | 0.4–0.5% | 0.4–0.5% |
Higher PC content reduces both the magnitude and the anisotropy of shrinkage — one reason PC/ABS is preferred for large, tight-tolerance parts.
4. Common Defects and Fixes
Most defects are visible within the first few shots, which makes them cheap to diagnose — as long as you know what you are looking at. The table below maps each symptom to its most likely cause and the corrective action, in rough order of likelihood.
Before working through it, note two diagnostics that save time. Part weight is the fastest indicator of whether the process is stable: a part that is light is under-filled or under-packed, a part that is heavy is over-packed. Weld-line location tells you where the flow fronts meet — write it down at first trial, because most weld-line strength problems are gate-location problems rather than parameter problems.
| Defect | Likely Cause | Fix |
| Silver streaks / splay | Moisture; contamination | Re-dry to ≤0.02%; check dew point; purge barrel |
| Weld line weakness | Low mold temperature, poor venting | Raise mold to 80–90 °C; add vents at weld lines; relocate gate |
| Warpage | Uneven cooling, excessive packing | Balance cooling circuits; reduce hold pressure; check gate position |
| Sink marks | Insufficient packing, thick ribs | Increase hold time and pressure; reduce rib thickness to ≤60% of wall |
| Short shots | Low melt temp, low injection speed, cold mold | Raise melt to 260–270 °C; increase speed; raise mold temp |
| Jetting | Undersized gate, high injection speed at gate | Enlarge gate; reduce initial injection speed (profile it) |
| Yellowing / burning | Melt too hot, long residence time, dead spots | Lower melt temp; reduce screw speed; check for material hang-up |
| Flow marks / tiger stripes | Low mold temp, inconsistent injection speed | Raise mold temp; profile injection speed; check check-ring wear |
| Stress cracking in service | Residual stress + chemical contact | Anneal at 80–90 °C for 2–4 h; eliminate incompatible chemicals |
| Black specks | Degraded material, worn screw/barrel | Purge thoroughly; inspect screw and barrel; reduce residence time |
5. Secondary Operations
Painting and printing. PC/ABS takes paint, pad printing, and laser marking well. Test the solvent carrier first — aggressive solvents cause stress cracking, especially on a stressed part. Anneal before painting, not after.
Electroplating. Standard PC/ABS is not plating-grade. Only high-butadiene plating grades can be electroplated. If you need a chrome finish, use plating-grade ABS.
Ultrasonic welding. PC/ABS welds well to itself and to ABS. It is not directly compatible with PC or PMMA without an energy-director redesign.
Laser welding. Some grades come in laser-transparent / laser-absorbing pairs for through-welding, useful for hermetically sealed enclosures.
Annealing. This is the most underused fix for PC/ABS field failures. Molded-in residual stress is the root cause of most environmental stress cracking, and annealing at 80–90 °C for 2–4 hours can improve ESC resistance by two to three times. Support the part to prevent sag and cool it slowly in the oven.
Assembly stress. A part can pass every molding check and still fail in the field because assembly introduced stress. Over-torqued screws, press-fit inserts without adequate boss wall thickness, and snap fits designed with insufficient strain allowance all create local stress concentrations that later become cracks. Design bosses with wall thickness of 60–70% of the nominal wall, specify torque limits, and keep snap-fit strain below 1.5% for PC/ABS at room temperature. These are design decisions, but they are made with the material’s properties in mind — review them before the tool is cut.
6. Regrind Management
PC/ABS tolerates regrind at low percentages, but impact strength drops faster than any other property.
| Regrind Level | Effect on Notched Izod | Recommendation |
| 0% (virgin) | Baseline | Cosmetic, structural, safety-critical parts |
| 10–15% | −5 to −10% | Acceptable for most non-cosmetic parts |
| 15–25% | −15 to −30% | Only with re-stabilization and impact modifier top-up |
| >25% | −30%+ and inconsistent | Not recommended without full requalification |
Always dry regrind as carefully as virgin material, and blend it uniformly. Inconsistent regrind blending is the number-one cause of lot-to-lot property variation in recycled PC/ABS.
Measuring regrind impact loss. Do not trust the visual appearance of a reground part. Verify impact retention with notched Izod testing to ISO 180 (or Charpy to ISO 179) on parts molded from each regrind level. A part can look perfect and still have lost 25% of its impact strength. For parts with a drop-test requirement, re-run the drop test itself on regrind-containing samples.
7. Process Monitoring and Quality Control
A PC/ABS run that is drifting can go out of specification before a defect becomes visible. Monitor these parameters continuously and record them per lot.
| Parameter | Target | Method | Alarm Condition |
| Moisture content | ≤0.02% | Karl Fischer or moisture analyzer | >0.03% |
| Melt temperature | 240–275 °C | Machine nozzle probe | Outside window |
| Mold temperature | 60–90 °C | Mold surface pyrometer | <60 °C or >95 °C |
| Injection pressure | 80–140 MPa | Machine controller | Trend rising (gate freezing) |
| Cushion | 3–8 mm | Machine controller | <2 mm or >10 mm |
| Cycle time | Stable | Machine controller | Drift >5% |
| Part weight | ±1% | Balance, per cavity | Drift >1.5% |
Part weight is the single best proxy for process stability. If part weight drifts, something in the process has changed — usually moisture, temperature, or check-ring wear. Track it per cavity, not per shot.
7.1 Verifying the Material, Not Just the Process
Even a perfect process cannot fix out-of-spec material. Confirm the incoming lot against the TDS using the material’s own tests:
| Property | Test Standard | Typical Acceptance |
| Density | ISO 1183 | Within TDS range |
| Melt flow rate | ISO 1133 | Within TDS range |
| Notched Izod | ISO 180 | ≥ TDS minimum |
| HDT | ISO 75-2 | ≥ TDS minimum |
| Glass transition (ratio check) | ISO 11357-2 (DSC) | Confirms PC content |
If a lot molds differently from the previous lot with identical parameters, suspect the material before you touch the machine. Density and DSC are the fastest way to confirm whether the ratio has drifted.
8. Frequently Asked Questions
What is the drying temperature for PC/ABS?
90–110 °C for 3–4 hours in a desiccant dryer, targeting ≤0.02% moisture. Never exceed 120 °C, or the ABS phase will degrade.
What is the melt temperature for PC/ABS?
240–275 °C. Start around 255–260 °C and adjust based on flow length and part appearance.
What mold temperature should I use?
60–70 °C for non-cosmetic parts, 80–90 °C for cosmetic Class-A surfaces and maximum impact retention. Running the hot side of the window is almost always worth it.
Why do my PC/ABS parts have silver streaks?
Silver streaks are almost always moisture. Re-dry to ≤0.02%, verify dryer dew point is ≤ −20 °C, and check that the material path from dryer to machine is sealed.
Can I mold PC/ABS in a mold designed for ABS?
Usually yes, with parameter changes — but check the gates and cooling. PC/ABS needs larger gates and more cooling capacity than ABS because of its higher viscosity. If the ABS mold has pin-point gates, they may be too restrictive.
Why do my PC/ABS parts crack after assembly or in a warehouse?
This is environmental stress cracking: residual molded-in stress plus contact with a chemical (mold release, adhesive, cleaner, solvent, or even skin oils). Anneal the parts at 80–90 °C for 2–4 hours and eliminate the offending chemical.
What regrind percentage is safe?
Up to 10–15% for non-cosmetic parts, with impact strength verified against ISO 180. Above 15%, only with re-stabilization. Never use regrind for safety-critical or cosmetic parts without requalification.
Why does my part weight keep drifting even though the parameters are locked?
Part weight drift almost always traces to one of four causes: moisture content rising (check the dryer), check-ring wear letting melt slip back, heater band failure, or incoming material with a different ratio. Measure moisture and density first — they are the fastest to rule out.
Can I run PC/ABS on a machine that was running ABS?
Yes, but purge thoroughly. PC/ABS runs 20–35 °C hotter than ABS, and residual ABS left in dead spots will degrade and appear as black specks. Use a proper purge compound, not just virgin PC/ABS.
What is the maximum residence time for PC/ABS in the barrel?
Keep residence time under about 8–10 minutes at 260–275 °C. Longer residence time at high temperature degrades the ABS phase and yellows the part. Match shot size to barrel capacity — a shot using less than 20% of barrel capacity means excessive residence time.
Should I profile the injection speed?
Yes, for cosmetic parts. A slow initial fill reduces jetting and gate blush; a fast main fill avoids hesitation marks and short shots; a slow final fill reduces over-packing near the gate. Profiling is one of the highest-return adjustments available and costs nothing to implement.
[Request Processing Support →] | [Ask for an Equivalent Grade Quote →]
Related Reading
- PC/ABS Blend: The Complete Guide to Properties, Grades and Applications
- PC/ABS vs ABS vs PC: Which One for Your Enclosure?
- PC/ABS Ratio Explained: How the PC:ABS Blend Ratio Changes Performance
- Flame-Retardant PC/ABS: UL94 V-0 Grades for IT and EV Housings
- Polycarbonate (PC): Properties, Grades and Applications