Most PC/ABS data sheets are written to hide the one number that matters. They list impact, HDT, and melt flow without ever stating the PC:ABS ratio, because a supplier selling a 40:60 blend at a 65:35 price does not want you to know the difference. This article explains what the ratio actually controls, how to estimate it, and how to specify it correctly.
1. What the Ratio Physically Controls
PC/ABS is a two-phase blend: a continuous PC phase with dispersed ABS domains (or the inverse at high ABS content). The ratio determines which phase dominates the material’s behavior.
- PC phase → contributes impact strength, heat resistance, stiffness, and dimensional stability. It is expensive and has a stiff, high-viscosity melt.
- ABS phase → contributes flow, surface finish, colorability, and cost reduction. It is cheaper and processes easily.
As PC content rises, the blend shifts from “processable but weak” toward “tough but difficult to mold.” There is no free lunch — every point of PC you add buys toughness and heat at the cost of flow and money.
Understanding the two-phase morphology explains why the properties move the way they do. In a low-PC blend, the ABS phase forms the continuous matrix and the PC domains are the dispersed phase; the material behaves much like ABS with a stiffening and toughening filler. As PC content rises past roughly 50%, the phases begin to co-continue, and above 60% the PC phase becomes dominant. The transition region — around 50–60% PC — is where small changes in ratio produce the largest changes in properties, which is also why it is the region where lot-to-lot consistency matters most. A supplier who runs “about 55%” with poor process control can swing 5 points of PC content between lots, which translates to a 20–30% swing in notched impact strength.
There is one more consequence worth knowing: the two phases degrade at different rates during processing. The ABS phase is more thermally sensitive, so a blend processed at the high end of the temperature window loses part of its ABS contribution first, and the resulting part behaves as though it has a higher PC content than its nominal ratio — stiffer, more brittle, and more notch-sensitive than the TDS suggests.
2. Property vs Ratio: The Full Curve
The table below shows how properties move as PC content increases. Values are typical for general-purpose unfilled grades; confirm against the specific grade TDS.
| PC Content | Notched Izod 23 °C (J/m) | HDT @1.82 MPa (°C) | MFR (260 °C/5 kg) | Density (g/cm³) | Relative Cost | Processability |
| 40% | 300–450 | 95–105 | 20–30 | 1.10–1.12 | Low | Excellent |
| 50% | 400–550 | 100–110 | 15–25 | 1.11–1.13 | Low–Med | Very good |
| 60% | 500–700 | 105–118 | 10–20 | 1.13–1.15 | Medium | Good |
| 70% | 650–800 | 112–125 | 8–15 | 1.14–1.16 | Med–High | Fair |
| 80% | 700–900 | 118–130 | 6–12 | 1.15–1.17 | High | Difficult |
Reading the table:
- Impact strength rises steeply between 40% and 60% PC, then flattens. This is why 60:40 is the most common commercial ratio — you capture most of the toughness benefit without paying the full PC premium.
- HDT climbs almost linearly with PC content. If heat resistance is your driver, ratio is your lever.
- Melt flow falls monotonically. At 80% PC, you are essentially molding PC with a slight flow aid, and thin-wall filling becomes a real challenge.
3. Choosing Your Ratio by Application
| Application | Recommended PC Content | Why |
| Large cosmetic enclosure, long flow | 45–55% | Flow and cost dominate; impact requirement is moderate |
| General electronics housing | 55–60% | Balanced toughness, flow, and finish |
| Thin-wall portable device housing | 60–65% | Drop-test impact mandatory at low temperature |
| Automotive interior trim | 55–65% | Heat aging + low-VOC + impact |
| Power tool housing | 60–70% | High impact, moderate heat, thick walls |
| Structural bracket or frame | 70–80% | Stiffness and heat under sustained load |
| Under-hood or high-heat part | Not recommended | Use PBT, PA, or PPS instead |
Practical default: If you have no data and no time, specify 60:40 PC:ABS with a notched Izod ≥500 J/m at 23 °C and an HDT ≥110 °C at 1.82 MPa. That covers the majority of enclosure applications and is the most widely available ratio.
4. How to Verify the Ratio You Are Actually Buying
Because suppliers rarely publish the ratio, you need a way to check. Three methods, in order of rigor.
4.1 Differential Scanning Calorimetry (DSC)
PC is amorphous with a glass transition temperature (Tg) of about 145–150 °C. ABS shows a much weaker Tg around 105–110 °C. In a DSC trace of PC/ABS, the PC Tg appears as a distinct step-change whose magnitude scales with PC content. Comparing the step height against calibrated reference blends gives an estimate good to roughly ±5%. Test method reference: ISO 11357-2 (plastics — DSC — determination of glass transition temperature). This is the standard method, and any compounder should be able to supply a DSC trace.
| DSC Parameter | Typical Value (PC/ABS ≈60:40) | Test Standard |
| PC Tg (onset) | 143–148 °C | ISO 11357-2 |
| ABS Tg (weak) | 103–110 °C | ISO 11357-2 |
| ΔCp step magnitude | Proportional to PC content | ISO 11357-2 |
| Estimated ratio accuracy | ±5% | — |
4.2 Thermogravimetric Analysis (TGA)
TGA measures weight loss as temperature rises. PC and ABS degrade at different temperatures and leave different residue profiles, so the decomposition curve can be deconvoluted to estimate composition. Test method reference: ISO 11358 (plastics — TGA of polymers). TGA is more useful for filled or flame-retardant grades where the DSC signal is muddied by additives.
4.3 Density and HDT Cross-Check
PC density is ~1.20 g/cm³ (ISO 1183); ABS is ~1.05 g/cm³. A measured density between those bounds gives a rough ratio estimate — but fillers, impact modifiers, and flame retardants all shift density, so use this only as a sanity check. Cross-check against HDT at 1.82 MPa (ISO 75-2) and notched Izod at 23 °C (ISO 180): if the density suggests a ratio that the HDT and impact values do not support, the material contains additives or is out of specification.
| Verification Method | Test Standard | Strength | Limitation |
| DSC | ISO 11357-2 | Direct ratio estimate, ±5% | Signal weak in filled/FR grades |
| TGA | ISO 11358 | Works on filled grades | Requires curve deconvolution |
| Density | ISO 1183 | Fast, cheap | Confounded by additives |
| HDT cross-check | ISO 75-2 | Confirms thermal performance | Indirect |
| Notched Izod | ISO 180 | Confirms impact performance | Indirect |
Red flag: A supplier who cannot provide a DSC trace, cannot state the ratio, and whose density is inconsistent with any single ratio is almost certainly selling an uncontrolled blend. Lot-to-lot variation in such material is the hidden cause of most “the part used to mold fine” complaints.
5. What Changes Beyond the Ratio
The ratio is primary, but three secondary factors can shift properties by as much as a 10-point ratio change:
Compatibilizer. A good PC/ABS blend includes a compatibilizer (often SAN-based or a grafted rubber) that controls domain size and interfacial adhesion. Two blends at the same ratio can differ by 30% in impact strength depending on compatibilization. This is where branded grades earn their premium.
Impact modifier. MBS or acrylic impact modifiers top up low-temperature toughness, especially in high-ABS blends. If your part must pass a −30 °C drop test, the modifier matters as much as the ratio.
Stabilizer package. UV stabilizers, antioxidants, and (for FR grades) the flame-retardant system all consume part of the property budget. A 60:40 blend with a heavy FR package can underperform a 55:45 blend with a light one.
| Secondary Factor | Typical Effect | When It Matters Most |
| Compatibilizer quality | ±30% on notched Izod | Any impact-critical part |
| Impact modifier | +50–100% at −30 °C | Cold drop tests |
| FR package | −10 to −25% on impact | UL94 V-0 parts |
| UV stabilizer | Slows yellowing 3–5× | Outdoor parts |
| Colorant | Small, but can embrittle | Dark or highly filled colors |
6. Cost vs Ratio: Where the Optimum Sits
| PC Content | Pellet Cost Index | Impact @23 °C | Cost per Unit Toughness |
| 40% | 100 | Low | Poor (you are buying flow, not strength) |
| 50% | 112 | Medium | Good |
| 60% | 125 | High | Best |
| 70% | 138 | Very high | Fair |
| 80% | 152 | Very high | Poor (diminishing returns) |
The cost-per-unit-toughness curve bottoms out around 55–65% PC. Above 70%, you are paying a steep price for incremental impact, and you are making the part harder to mold at the same time. Unless heat resistance specifically demands it, there is rarely a commercial reason to go above 70% PC.
7. Ratio vs Processing Window
The ratio does not only change properties — it changes how you have to run the machine. Higher PC content means higher melt viscosity, which means higher temperatures, higher pressures, and a narrower window.
| Parameter | 40:60 | 60:40 | 70:30 |
| Melt temperature (°C) | 230–260 | 240–275 | 250–285 |
| Mold temperature (°C) | 50–75 | 60–90 | 70–95 |
| Injection pressure (MPa) | 70–120 | 80–140 | 90–150 |
| Drying temperature (°C) | 85–100 | 90–110 | 95–115 |
| Drying time (h) | 2–3 | 3–4 | 3–5 |
| Shrinkage (%) | 0.5–0.7 | 0.4–0.6 | 0.4–0.5 |
| Wall thickness minimum (mm) | 1.0 | 1.2 | 1.4 |
If you switch to a higher-PC grade without adjusting parameters, you will see short shots and high molded-in stress. If you switch to a lower-PC grade and keep the old, hotter parameters, you risk degrading the ABS phase. Always re-run the process window when the ratio changes — even within the same supplier’s grade family.
8. Frequently Asked Questions
What is the most common PC/ABS ratio?
About 60:40 PC:ABS is the most widely specified ratio. It captures most of the toughness and heat benefit of PC while keeping flow and cost within reason.
How do I know the ratio without a DSC trace?
You largely cannot. Density and HDT give rough bounds, but both are confounded by additives. If your supplier will not supply a DSC trace, treat the material as unqualified for any application where impact or heat is critical.
Does a higher PC content always mean better?
No. Higher PC means higher impact and heat but also higher cost, lower flow, worse chemical resistance, and more notch sensitivity. The right ratio is the lowest one that meets your drop and heat requirements.
Can I blend PC and ABS myself to change the ratio?
Technically yes, but only with a compatibilizer and a twin-screw compounding line. Simply dry-blending PC and ABS pellets produces a material with poor interfacial adhesion and unpredictable impact strength. Do not attempt this without proper compounding equipment.
Why does my 60:40 part behave differently from another supplier’s 60:40 part?
Because “60:40” alone says nothing about compatibilization, impact modifier, or stabilizer package. Two 60:40 blends from different compounders can differ by 30% in impact strength.
What ratio should I specify for a low-temperature drop test?
For a −30 °C drop test, specify ≥65% PC with a documented low-temperature impact modifier, and require notched Izod at −30 °C on the TDS (ISO 180). Ratio alone is not sufficient — the modifier system is doing much of the work.
Does the ratio affect regrind tolerance?
Yes. Higher-PC blends lose impact strength faster on repeated processing because the PC phase is more sensitive to thermal history. Keep regrind below 15% for blends above 60% PC, and below 25% for blends at or below 50% PC.
How much does the ratio affect dimensional stability?
Materially. Higher PC content reduces both the magnitude and the anisotropy of shrinkage (see the shrinkage row above). For a large, tight-tolerance part, this alone is often the reason to specify a higher-PC ratio.
Can two grades with the same ratio have different properties?
Yes, significantly. Compatibilizer quality, impact modifier system, and stabilizer package can swing notched impact strength by 30% or more at an identical ratio. Ratio is necessary but not sufficient to describe a grade.
9. Specifying Ratio in a Purchase Order
Put the ratio in writing. A specification that says “PC/ABS, general purpose” is not a specification. Use this checklist:
| Item | Example Specification |
| Ratio | PC:ABS 60:40, verified by DSC (ISO 11357-2) |
| Notched Izod, 23 °C | ≥500 J/m (ISO 180) |
| Notched Izod, −30 °C | ≥120 J/m (ISO 180) |
| HDT at 1.82 MPa | ≥110 °C (ISO 75-2) |
| Density | 1.13–1.15 g/cm³ (ISO 1183) |
| Melt flow rate | 10–20 g/10 min (ISO 1133, 260 °C/5 kg) |
| Documentation | TDS, DSC trace, COA per lot |
If a supplier resists putting the ratio in writing, that is itself the answer. A compounder who controls their blend can state the ratio confidently; one who buys generic compound on the spot market cannot.
What to do when the ratio drifts. If incoming inspection shows the ratio has moved — density or DSC outside the specified window — do not simply adjust the process to compensate. A ratio drift changes impact and heat performance, and a process adjustment cannot restore either. Quarantine the lot, request the supplier’s batch record, and require re-verification before the material enters production. Compensating for a material defect with a process change is how a marginal lot becomes a field failure.
10. Next Steps
Specify PC/ABS by ratio, not by brand name or generic grade number. Write the ratio, the notched Izod at both 23 °C and −30 °C, and the HDT at 1.82 MPa into your specification, and require a DSC trace on every lot.
Because we compound in-house, we can produce PC/ABS at any ratio from 40:60 to 80:20, with the compatibilizer and impact modifier system tuned to your application. If your current grade is underperforming on a cold drop test or over-specifying on heat, we can adjust the ratio to find the optimum rather than selling you a fixed catalog number.
What we can send you:
- PC/ABS samples at any ratio in the 40:60–80:20 range
- DSC traces and TDS confirming composition
- COA with batch traceability
- Trial quantities for your own drop and heat testing
[Request a Custom-Ratio Sample →] | [Ask for an Equivalent Grade Quote →]
Related Reading
- PC/ABS Blend: The Complete Guide to Properties, Grades and Applications
- PC/ABS vs ABS vs PC: Which One for Your Enclosure?
- PC/ABS Processing Guide: Drying, Melt Temperature and Mold Design
- PC/PBT Alloy: Properties, Chemical Resistance and Applications
- Flame-Retardant PC/ABS: UL94 V-0 Grades for IT and EV Housings
- Polycarbonate (PC): Properties, Grades and Applications