All three are amorphous styrenic or polycarbonate-based thermoplastics, but they sit at different points on the performance-cost curve.
ABS is the commodity choice — cheap, easy to mold, plateable, limited to about 80 °C. PC is the performance choice — highest impact, highest heat resistance, transparent, and the most expensive and hardest to process. PC/ABS occupies the commercially dominant middle: about 2–3× ABS’s impact strength, 20–40 °C more heat resistance, and processability close enough to ABS that most tools can be adapted. For engineering applications, PC/ABS is the default unless a specific requirement rules it out.
This article approaches the comparison from an engineering-selection standpoint rather than a properties-only view.
1. Where Each Material Sits in the Engineering Plastics Landscape
Engineering plastics are defined by their ability to bear structural load and resist heat — a tier above commodity resins like PP, PS, and PE. Within that tier, these three occupy distinct positions.
It is worth being precise about the tiers, because the labels influence expectations. The engineering plastics category is usually divided into three bands: commodity-adjacent resins that are cheap and easy to process (ABS, SAN, PMMA); workhorse engineering resins that carry structural load at moderate temperature (PC/ABS, PBT, PA, POM); and high-performance resins that carry load at high temperature (PEEK, PPS, PEI, PSU). The three materials in this article span the first two bands, with PC straddling the boundary — its heat resistance reaches into territory that most workhorse engineering resins cannot.
The practical significance: if a requirement pushes beyond PC’s ceiling of roughly 120 °C continuous service, none of these three will do, and the conversation moves to PBT, PA, PPS, or PEI. Knowing where the ceiling is prevents a very common error — trying to solve a high-temperature problem with PC/ABS or PC when the correct answer is a different material family entirely.
| Position | Material | Character |
| Commodity-adjacent | ABS | Low cost, high processability, moderate performance |
| Workhorse engineering | PC/ABS | Balanced performance-cost, dominant in enclosures |
| High-performance engineering | PC | Peak impact and heat, higher cost and process demand |
The tier matters because it sets expectations. ABS is the entry point to structural plastics; PC/ABS is where most commercial engineering designs land; PC is where the requirements exceed what the alloy can deliver.
1.1 A Note on “Engineering Plastic”
The term is used loosely. Strictly, ABS is a styrenic commodity resin; PC is an engineering plastic; PC/ABS is an engineering alloy. In practice, all three compete for the same applications — enclosures, housings, structural covers — so treating them as a single selection set is the right approach for a design engineer.
1.2 The Cost-Performance Curve
The most useful mental model for this comparison is a cost-performance curve with three points on it. ABS sits at the low-cost, moderate-performance end. PC sits at the high-cost, high-performance end. PC/ABS sits between them — but not at the midpoint. It sits closer to the performance end than the cost end, which is why it dominates the middle of the market.
| Material | Relative Cost | Relative Impact | Relative Heat | Value Position |
| ABS | 1.0× | 1.0× | 1.0× | Entry point |
| PC/ABS | 1.25–1.35× | 2–3× | 1.3× | Best value in the set |
| PC | 1.55–1.80× | 4–5× | 1.5× | Premium |
The “value” column is the reason PC/ABS is the default for engineered enclosures. Moving from ABS to PC/ABS buys a 100–200% improvement in impact for a 25–35% cost increase — an excellent trade. Moving from PC/ABS to PC buys roughly another 50% improvement in impact for a similar cost increase — a much poorer trade, justified only when a specific requirement demands it (transparency, or a heat load PC/ABS cannot carry).
How to use this in a design review. When someone proposes PC where PC/ABS would do, the question to ask is: which requirement does PC satisfy that PC/ABS does not? If the answer is transparency or a temperature above 125 °C, PC is right. If the answer is “it’s better,” the specification is being driven by a data sheet rather than a requirement, and it is costing more than it needs to.
2. The Full Comparison Table
| Property | ABS | PC/ABS (≈60:40) | PC | Test Standard |
| Density (g/cm³) | 1.04–1.07 | 1.10–1.16 | 1.19–1.22 | ISO 1183 |
| Notched Izod, 23 °C (J/m) | 150–350 | 400–800 | 600–900 | ISO 180 |
| Notched Izod, −30 °C (J/m) | 60–120 | 100–250 | 200–400 | ISO 180 |
| Tensile strength (MPa) | 40–50 | 50–62 | 60–70 | ISO 527 |
| Tensile modulus (MPa) | 2,000–2,500 | 2,100–2,500 | 2,300–2,500 | ISO 527 |
| Flexural modulus (MPa) | 2,000–2,500 | 2,200–2,600 | 2,300–2,500 | ISO 178 |
| HDT at 1.82 MPa (°C) | 80–95 | 100–125 | 128–138 | ISO 75-2 |
| HDT at 0.45 MPa (°C) | 90–105 | 110–135 | 135–143 | ISO 75-2 |
| Vicat softening (°C) | 95–105 | 110–130 | 140–155 | ISO 306 |
| Melt flow rate | 15–40 (220/10) | 8–25 (260/5) | 4–15 (300/1.2) | ISO 1133 |
| Shrinkage (%) | 0.4–0.7 | 0.4–0.7 | 0.5–0.7 | ISO 2577 |
| Water absorption 24 h (%) | 0.2–0.5 | 0.2–0.4 | 0.15–0.35 | ISO 62 |
| Dielectric strength (kV/mm) | 15–25 | 15–25 | 15–35 | IEC 60243 |
| Transparency | No | No | Yes (natural) | — |
| Electroplating | Excellent | Poor | Poor | — |
| UV stability (unmodified) | Poor | Poor | Poor | — |
| Relative cost | $ | $$ | $$$ | — |
The rows that decide most projects are notched Izod, HDT at 1.82 MPa, and transparency. Everything else is secondary for enclosure work.
3. Property-by-Property Analysis
The comparison table gives the numbers; this section explains what they mean for a design decision. The three properties that decide most projects are impact strength, heat resistance, and transparency — so those come first.
The general pattern to internalize is that the performance curve between these materials is not linear in cost. Moving from ABS to PC/ABS costs 25–35% more and buys roughly 2–3× the impact strength and 20–40 °C more heat resistance. Moving from PC/ABS to PC costs another 25–35% and buys considerably less incremental improvement — perhaps 30% more impact and 15 °C more heat, depending on grade. This is why PC/ABS captures the middle of the market so thoroughly: it sits on the steep part of the performance curve, where each unit of cost buys the most benefit.
3.1 Impact Strength
| Material | Notched Izod 23 °C | Relative |
| ABS | 150–350 J/m | 1× (baseline) |
| PC/ABS | 400–800 J/m | 2–3× |
| PC | 600–900 J/m | 4–5× |
The step from ABS to PC/ABS is much larger than the step from PC/ABS to PC. This is the fundamental commercial fact about the alloy: it captures most of the toughness benefit of PC at a fraction of the cost difference. That is why PC/ABS dominates enclosures and ABS is confined to cost-driven, low-demand parts.
Cold impact is where the difference becomes sharpest. At −30 °C, ABS retains only 40–50% of its room-temperature impact, PC/ABS retains about 25–40%, and PC retains 30–45% but from a much higher starting point.
3.2 Heat Resistance
| Material | HDT @1.82 MPa | Continuous Service (approx.) |
| ABS | 80–95 °C | ~70 °C |
| PC/ABS | 100–125 °C | ~95 °C |
| PC | 128–138 °C | ~120 °C |
The practical meaning: ABS fails in a hot car interior (dashboards reach 90–110 °C in direct sun). PC/ABS survives it. PC survives it with margin and also handles some under-hood and electronics environments that PC/ABS cannot.
3.3 Processability
| Material | Ease of Molding | Melt Temp | Mold Temp | Drying |
| ABS | Easiest | 220–260 °C | 50–80 °C | 2–3 h @ 80–90 °C |
| PC/ABS | Moderate | 240–275 °C | 60–90 °C | 3–4 h @ 90–110 °C |
| PC | Hardest | 280–310 °C | 80–110 °C | 4–6 h @ 110–120 °C |
ABS’s processability advantage is real: wider window, faster cycles, lower temperatures, less drying. PC/ABS narrows that advantage but remains within reach of most ABS tools. PC requires the most process discipline and often a machine with adequate shot capacity.
3.4 Chemical and Environmental Resistance
All three are vulnerable to solvents, fuels, and aggressive cleaners, and all three undergo environmental stress cracking when stress and chemical contact combine. The differences are modest and not usually decisive:
| Medium | ABS | PC/ABS | PC |
| Alcohols | Fair | Fair–Poor | Poor |
| Aliphatic hydrocarbons | Poor | Poor | Poor |
| Aromatic solvents | Poor | Poor | Poor |
| Dilute acids | Good | Good | Good |
| Dilute bases | Good | Fair | Poor (hydrolyzes) |
| Detergents (with stress) | Moderate ESCR | Moderate ESCR | Poor ESCR |
If chemical resistance is the driving requirement, none of these three is the right family — look at PC/PBT or PBT instead.
3.5 Transparency
Only PC offers transparency in its natural form. ABS and PC/ABS are opaque. If the part must be clear, PC is the only candidate among the three; for optical precision, PMMA may be better still (see PC vs PMMA).
3.6 Electrical Properties
All three are good electrical insulators, and the differences between them are rarely decisive for standard applications.
| Property | ABS | PC/ABS | PC |
| Dielectric strength (kV/mm) | 15–25 | 15–25 | 15–35 |
| Volume resistivity (Ω·cm) | 10¹⁵–10¹⁶ | 10¹⁵–10¹⁶ | 10¹⁵–10¹⁷ |
| CTI (V) | 250–600 | 250–600 | 250–600 |
| Dielectric constant (1 MHz) | 2.8–3.2 | 2.9–3.2 | 2.9–3.0 |
For flame-retardant versions, the FR package dominates the electrical behavior — see our FR PC/ABS guide for glow-wire and CTI considerations. PC’s slightly higher dielectric strength is occasionally useful in high-voltage insulation, but where electrical performance is the primary requirement, a purpose-formulated grade (FR, high-CTI) matters far more than the base polymer choice.
3.7 Weatherability
None of the three performs well outdoors in unmodified form, and this is one of the few areas where the ranking is essentially flat.
| Material | Unmodified Outdoor Life | Notes |
| ABS | 6–18 months | Butadiene phase degrades; yellowing and embrittlement |
| PC/ABS | 6–18 months | Same butadiene mechanism |
| PC | 1–3 years | Yellows; embrittles; needs UV package |
The correct answer for outdoor service is not to choose among these three but to move to a material designed for it — PC/ASA for rigid outdoor parts, ASA for profile and cladding applications, or PMMA for transparent outdoor panels. Adding a UV package to ABS or PC/ABS extends life but does not match these alternatives.
4. Selection Framework
Step 1 — Must the part be transparent? Yes → PC. No → continue.
Step 2 — Will the part exceed 120 °C in continuous service? Yes → PC. No → continue.
Step 3 — Must the part pass a drop test, or operate between 90 °C and 120 °C? Yes → PC/ABS. No → continue.
Step 4 — Must the part be electroplated? Yes → ABS (plating grade). No → continue.
Step 5 — Is the part cost-driven with a ceiling below 80 °C? Yes → ABS. No → PC/ABS as the engineered default.
4.1 Application Mapping
| Application | Temperature | Impact | Plating | Material |
| Laptop bottom housing | Medium | High | No | PC/ABS |
| Monitor bezel | Low–Med | Low | No | ABS or PC/ABS |
| Automotive IP carrier | High | Medium | No | PC/ABS (low-VOC) |
| Machine guard | Low | Very high | No | PC |
| Optical lens | Low | Varies | No | PC |
| Appliance knob (chrome) | Low | Low | Yes | ABS (plating) |
| Power tool housing | Medium | High | No | PC/ABS |
| Safety helmet shell | Medium | Very high | No | PC (opaque) or PC/ABS |
| Cost-driven bracket | Low | Low | No | ABS |
| EV charger cover | High | Medium | No | FR PC/ABS or PC/ASA |
5. Cost Analysis
| Factor | ABS | PC/ABS | PC |
| Pellet cost index | 100 | 125–135 | 155–180 |
| Scrap rate (thin wall) | Low | Medium | High |
| Cycle time index | 100 | 110–115 | 125–135 |
| Tool modification from ABS | — | Minor | Significant |
| Drying/process overhead | Low | Medium | High |
| Field-failure risk (impact) | Higher | Low | Low |
Total cost of ownership usually favors PC/ABS for any part that is handled, shipped, or heated, because the field-failure risk of ABS outweighs its pellet-price advantage. For parts that are neither dropped nor heated, ABS is the correct economic choice.
A common costing error: comparing only pellet price and concluding PC/ABS is “35% more expensive.” A part that fails in the field costs the pellet premium many times over in returns, rework, and brand damage. When the application has impact or heat requirements, price the failure risk, not just the resin.
6. Substitution Between the Three
Changing material within this set is a real engineering decision, not a paperwork change.
The reason substitution is risky here is that these three materials have similar shrinkage and similar design conventions, which makes a switch look safe. A designer looking at the data sheets sees comparable densities, comparable shrinkage, and comparable processing behavior, and concludes that a substitution is a formality. It is not — the impact strength difference between ABS and PC/ABS is a factor of two to three, and between ABS and PC it is a factor of four to five. A part that passed its drop test on PC/ABS will not automatically pass on ABS, and the failure will occur in the field rather than on the bench.
| Direction | What Changes | What to Verify |
| ABS → PC/ABS | Impact up 2–3×, HDT up 20–40 °C | Tool adaptation (open gates, more cooling); shrinkage similar |
| ABS → PC | Impact up 4–5×, HDT up 40–50 °C | Significant tool changes; new process window; higher cost |
| PC/ABS → PC | Impact up ~30%, HDT up ~15 °C | Gating and cooling; notch sensitivity increases |
| PC → PC/ABS | Impact down ~30%, HDT down ~15 °C | Whether the original requirement still holds |
| PC/ABS → ABS | Impact down ~60%, HDT down ~30 °C | Re-validation of drop and heat tests mandatory |
| PC → ABS | Impact down ~80%, HDT down ~45 °C | Usually not viable for the original application |
The substitution rule: define the requirement, not the grade. If you are substituting because of cost or availability, write down the actual acceptance criteria — notched Izod at the service temperature, HDT, FR rating, color, finish — and qualify against those. Copying an incumbent grade number into a new material’s data sheet proves nothing.
7. Frequently Asked Questions
Is PC/ABS an engineering plastic?
Yes, in practice. PC/ABS is an engineering alloy that sits between ABS (commodity-adjacent) and PC (high-performance engineering). It is widely used for structural enclosures.
Which is stronger, ABS or PC/ABS?
PC/ABS on every structural measure: 2–3× the notched impact strength and 20–40 °C more heat resistance. ABS is “stronger” only in cost and processability.
Can I replace PC with PC/ABS to save cost?
Sometimes, but not automatically. PC/ABS has about 30% less impact strength and 15 °C less heat resistance. If the part passed its tests on PC, re-validate on PC/ABS before switching — especially drop tests and high-temperature dimensional checks.
Which of the three is easiest to mold?
ABS, then PC/ABS, then PC. If your tool was designed for ABS, running PC/ABS is usually feasible with parameter changes; running PC may require gating and cooling modifications.
Which has the best chemical resistance?
None of the three is strong here. They are broadly similar and all vulnerable to solvents and fuels. If chemical resistance is the requirement, look at PC/PBT or PBT.
Is PC/ABS or PC better for outdoor use?
Neither, unmodified. Both yellow and embrittle under UV. For outdoor service, specify PC/ASA or a UV-stabilized grade with documented weathering data.
Does PC/ABS cost much more than ABS?
Typically 25–35% more per kilogram. Whether that is worth it depends entirely on whether the part has an impact or heat requirement — if it does, PC/ABS almost always wins on total cost of ownership.
Which of the three should I specify if the part has no special requirements?
ABS, if cost genuinely dominates and there is no impact or heat demand. But most parts that look “ordinary” on paper do get dropped, shipped, or warmed in service, and those are exactly the requirements that favor PC/ABS. Audit the real service conditions before defaulting to the cheapest material.
8. Next Steps
For engineering selection among these three, the decision collapses to two questions: is the part dropped (impact) and does it get hot (temperature). If either answer is yes, PC/ABS. If the part must be clear or extreme heat applies, PC. If neither applies and cost dominates, ABS.
We supply ABS, PC, and PC/ABS across the full grade range — general-purpose, high-flow, flame-retardant, low-odor automotive, glass-filled, and custom alloys — and because we compound PC/ABS in-house, we can tune the ratio and additive package to your drop, heat, and finish requirements rather than selling you the nearest catalog grade.
What we can send you:
- TDS for all three materials for side-by-side comparison
- Samples for your own drop and heat testing
- UL yellow card copies for FR grades
- COA and batch traceability
- Substitution qualification support
[Request TDS and Samples →] | [Ask for an Equivalent Grade Quote →]
Related Reading
- Polycarbonate (PC): Properties, Grades and Applications
- PC/ABS Blend: The Complete Guide to Properties, Grades and Applications
- PC/ABS vs ABS vs PC: Which One for Your Enclosure?
- PC/ABS Alloy: Properties, Applications and Injection Molding
- PC vs PMMA (Acrylic): Optical Clarity, Impact and Cost
- PC/ABS Ratio Explained: How the PC:ABS Blend Ratio Changes Performance