Every enclosure project reaches the same fork in the road: ABS, PC, or the alloy in between. The wrong choice shows up months later as cracked corners in the field, warped covers that will not fit, or a part that simply costs more than it needed to. This guide gives you the comparison data to make the call on the first pass, with the trade-offs stated plainly.
1. The Three Materials in One Table
The fastest way to choose is to look at the numbers side by side. The table below uses typical unfilled, general-purpose grades.
| Property | ABS | PC/ABS (≈60:40) | PC |
| Density (g/cm³) | 1.04–1.07 | 1.10–1.16 | 1.19–1.22 |
| Notched Izod, 23 °C (J/m) | 150–350 | 400–800 | 600–900 |
| Notched Izod, −30 °C (J/m) | 60–120 | 100–250 | 200–400 |
| HDT at 1.82 MPa (°C) | 80–95 | 100–125 | 128–138 |
| HDT at 0.45 MPa (°C) | 90–105 | 110–135 | 135–143 |
| Tensile strength (MPa) | 40–50 | 50–62 | 60–70 |
| Flexural modulus (MPa) | 2,000–2,500 | 2,200–2,600 | 2,300–2,500 |
| Melt flow rate (g/10 min) | 15–40 (220 °C/10 kg) | 8–25 (260 °C/5 kg) | 4–15 (300 °C/1.2 kg) |
| Mold shrinkage (%) | 0.4–0.7 | 0.4–0.7 | 0.5–0.7 |
| Water absorption, 24 h (%) | 0.2–0.5 | 0.2–0.4 | 0.15–0.35 |
| Relative cost | $ | $$ | $$$ |
| Transparency | No | No | Yes (natural) |
| Electroplating | Excellent | Poor (needs special grade) | Poor |
| UV resistance (unmodified) | Poor | Poor | Poor |
| Test standards | ISO 1183 / 180 / 75-2 / 527 / 178 | ISO 1183 / 180 / 75-2 / 527 / 178 | ISO 1183 / 180 / 75-2 / 527 / 178 |
The single most important row is notched Izod at 23 °C: PC/ABS sits roughly 2–3× above ABS and about 70–90% of the way to PC. That is the entire commercial reason the alloy exists.
2. Where Each Material Wins
The comparison table tells you the numbers; this section tells you what they mean for a design. Each material has a domain where it is the objectively correct choice, and the fastest way to a good decision is to ask which domain your part falls into.
2.1 ABS Wins When: Cost, Flow, and Plating Drive the Decision
ABS is the workhorse of consumer plastic. It is cheap, flows beautifully into thin walls, takes a Class-A finish, and — uniquely among these three — electroplates exceptionally well.
Choose ABS when:
- The part is cost-driven and the volume is high (ABS is typically 20–35% cheaper per kilogram than PC/ABS)
- Wall sections are thin and flow length is long (ABS fills at lower pressure and lower temperature)
- The part needs a chrome or metallic finish (electroplating is an ABS specialty)
- Maximum continuous service temperature stays below ~80 °C
- Impact requirements are moderate — a hand-held device drop, not a stadium seat
Do not choose ABS when the part will sit on a dashboard, house a power supply, or be exposed to sustained loads near heat.
2.2 PC/ABS Wins When: You Need the Middle Ground
PC/ABS is the answer to the question “I need ABS’s processability and cost but ABS is not tough or heat-resistant enough.” It is the default for laptop housings, automotive interior trim, power tools, and EV charger covers precisely because no other single material covers impact, heat, finish, and processability at that price point.
Choose PC/ABS when:
- The part must pass a drop test (1 m at −20 °C is a common target)
- The part sees sustained heat between 90 °C and 120 °C
- The part has a large footprint and needs low, isotropic shrinkage to hold tolerances
- You need a paintable, laser-markable, Class-A surface
- You need flame retardancy (UL94 V-0) in a structural part — FR PC/ABS grades are well established, FR ABS less so
Watch out for: chemical exposure (solvents, adhesives, cleaners cause stress cracking), and UV (PC/ABS yellows outdoors — switch to PC/ASA).
2.3 PC Wins When: Clarity, Heat, or Maximum Impact Is Mandatory
PC is the strongest of the three, the most heat-resistant, and — in its natural form — optically clear. It is also the most expensive, the most notch-sensitive, and the hardest to mold.
Choose PC when:
- The part must be transparent (lenses, light guides, signage, protective visors)
- Continuous service temperature exceeds 120 °C
- Impact requirement is extreme (safety helmets, machine guards, riot shields)
- Dimensional stability over temperature is critical
Watch out for: PC is notch-sensitive — a sharp corner or a scratch can turn a tough part into a brittle one. Design generous radii, avoid sharp gate marks, and dry it thoroughly (PC hydrolyzes aggressively).
3. The Decision Framework
Work through these five questions in order. The first one that returns a “yes” usually decides the material.
Question 1 — Must the part be transparent? Yes → PC (or PMMA if scratch resistance matters more than impact; see PC vs PMMA). No → continue.
Question 2 — Will the part exceed 120 °C in service? Yes → PC (or a higher-temperature resin such as PBT, PA, PPS for under-hood). No → continue.
Question 3 — Must the part pass a drop test, or sit between 90 °C and 120 °C? Yes → PC/ABS. No → continue.
Question 4 — Does the part need electroplating? Yes → ABS (plating grade). No → continue.
Question 5 — Is the part cost-driven with service temperature below 80 °C? Yes → ABS. No → PC/ABS is the safe default.
The default rule: When uncertain between ABS and PC/ABS, and the part is opaque, structural, and will be handled or shipped, specify PC/ABS. The cost premium is small relative to the field-failure risk of a cracked ABS part.
4. Cost of Ownership: Pellet Price Is Not the Whole Story
The mistake teams make is comparing only the pellet price. Consider a laptop-bottom housing program:
| Cost Factor | ABS | PC/ABS | PC |
| Pellet cost per part | Baseline | +25–35% | +55–80% |
| Scrap rate (thin-wall, tight tolerance) | Low | Medium | High |
| Mold cost (flow, cooling, gating) | Lowest | Medium | Highest |
| Cycle time | Fastest | Medium | Slowest |
| Field failure / warranty risk | Higher | Low | Low |
| Drying / process control overhead | Low | Medium | High |
For a large thin-wall part, PC’s higher scrap rate and slower cycle can erase its per-kilogram disadvantage only if impact and heat demand it. For a drop-tested enclosure, PC/ABS’s lower warranty risk usually justifies its premium over ABS within the first production year.
Rule: Cost-driven commodity part → ABS. Anything that gets dropped, heated, or shipped assembled → PC/ABS. Optical or extreme-heat → PC.
5. Processing Comparison
All three are amorphous and hygroscopic, but they behave very differently at the machine. Moving a part from ABS to PC/ABS or PC is not a matter of changing the temperature setpoints — it changes drying time, cycle time, tool requirements, and the sensitivity of the process to small disturbances.
The practical consequences are worth spelling out. ABS is forgiving: it tolerates modest moisture, runs on a wide temperature window, and recovers quickly from a brief interruption. PC/ABS needs real drying and a hot mold, and it punishes shortcuts with visible defects. PC needs all of that plus higher pressures and a machine with enough shot capacity to avoid long residence times — and PC degrades visibly if residence time runs long.
| Parameter | ABS | PC/ABS | PC |
| Drying temperature (°C) | 80–90 | 90–110 | 110–120 |
| Drying time (h) | 2–3 | 3–4 | 4–6 |
| Target moisture (ppm) | ≤200 | ≤200 | ≤200 |
| Melt temperature (°C) | 220–260 | 240–275 | 280–310 |
| Mold temperature (°C) | 50–80 | 60–90 | 80–110 |
| Injection pressure (MPa) | 60–100 | 80–140 | 100–150 |
| Holding pressure (% of injection) | 40–60 | 40–70 | 50–70 |
| Screw speed | High | Moderate | Low |
| Nominal wall minimum (mm) | 0.8 | 1.2 | 1.5 |
| Regrind tolerance | High | Medium | Low |
| Moisture sensitivity | Moderate | High | Very high |
| Process window width | Wide | Medium | Narrow |
Two practical notes:
- Drying is where most failures start. All three hydrolyze, but PC is the most aggressive — a wet PC part loses impact strength permanently and cannot be recovered by re-melting. Never skip drying, and never trust a hot-air oven for PC or PC/ABS; you need a desiccant dryer with a dew point of ≤ −20 °C.
- Mold temperature drives surface and weld-line strength. Running a cosmetic PC/ABS or PC part at the cold end of the window produces dull surfaces, visible flow marks, and weak weld lines — even though the part may look acceptable on a quick visual check. Run the hot side for anything visible.
Machine selection. If you are moving a part from ABS to PC, check the injection unit’s shot capacity. A PC shot should use at least 20–25% of the barrel capacity, or the residence time will be long enough to degrade the material. Under-sized machines are a common reason a PC conversion “fails” in the first trial when the material itself is fine.
6. Real-World Selection Scenarios
Abstract property tables only get you so far. Here is how the decision plays out in five common projects.
6.1 Laptop Bottom Housing, Thin Wall, Drop-Tested
The part is 1.2 mm at the thinnest point, has a long flow path from a central gate, and must survive a 76 cm drop onto concrete at −20 °C. ABS flows well enough but fails the cold drop — its notched Izod at −30 °C is only 60–120 J/m, and the part cracks at the corner radii. Pure PC passes the drop but is difficult to fill at 1.2 mm and shows high scrap. PC/ABS at 60–65% PC wins, because it flows better than PC while retaining enough low-temperature impact to pass the corner-drop test.
6.2 Automotive Door Panel Carrier
The part sees 90–105 °C surface temperature in a parked car, must be low-odor and low-VOC, and must take an integrated clip without cracking. ABS’ HDT of 80–95 °C is marginal and it will creep under sustained clip load. PC alone is over-specified and expensive. PC/ABS with a low-odor/low-VOC grade at 55–65% PC is the standard answer.
6.3 Electroplated Appliance Control Knob
The part needs a chrome finish. Electroplating requires the butadiene-rich chemistry of plating-grade ABS — PC/ABS will not etch and plate properly even at high ABS content. Plating-grade ABS wins unambiguously, regardless of the impact or heat budget.
6.4 Safety Machine Guard
The guard is a flat transparent or opaque panel exposed to impact from ejected parts. Clarity may or may not be required, but impact always is. PC wins — its notched Izod is 600–900 J/m versus 400–800 J/m for PC/ABS and 150–350 J/m for ABS, and PC has the highest ductile-brittle transition margin.
6.5 Cost-Sensitive Consumer Enclosure, No Heat, No Drop
A wall-mounted bracket for a low-power device, never dropped, never above 60 °C, produced in high volume. ABS wins — it is 20–35% cheaper per kilogram and molds faster. Specifying PC/ABS here is simply paying for properties the part never uses.
| Scenario | Impact Needed | Heat Needed | Plating | Winner |
| Laptop bottom, cold drop | High | Medium | No | PC/ABS (60–65% PC) |
| Automotive door carrier | Medium | High | No | PC/ABS (low-VOC) |
| Electroplated knob | Low | Low | Yes | Plating-grade ABS |
| Safety machine guard | Very high | Low–Med | No | PC |
| Cost-driven bracket | Low | Low | No | ABS |
6.6 A Note on “Just Use the Best One”
A common shortcut is to specify PC everywhere because it has the highest numbers. This is almost always a mistake, and it costs more than it saves. PC’s higher melt viscosity means more scrap on thin walls, its higher price means more material cost on every part, and its notch sensitivity means a design that was safe in ABS can fail in PC at a sharp corner. The material with the best data sheet is not the material with the best economics. Match the material to the requirement, not to the ranking.
7. Frequently Asked Questions
Is PC/ABS stronger than ABS?
Yes — on impact strength, PC/ABS is typically 2–3× more impact-resistant than ABS, and its heat deflection temperature is 20–40 °C higher. ABS is only “stronger” in the sense of being cheaper and easier to process.
Is PC/ABS the same as PC?
No. PC is a single polymer; PC/ABS is an alloy of PC and ABS. PC offers higher heat resistance, higher impact strength, and transparency. PC/ABS offers better flow, lower cost, and better colorability, and it is less notch-sensitive.
Can I use ABS where I currently use PC/ABS?
Only if you re-validate. Moving to ABS will reduce impact strength by roughly half and lower the heat deflection temperature by 20–40 °C. If the part passed its drop and heat tests on PC/ABS, it will not automatically pass on ABS.
Which is better for an outdoor enclosure?
None of the three, in unmodified form. UV degrades all of them. For outdoor parts, specify PC/ASA (which retains color and impact under UV and humidity) or a UV-stabilized grade with a documented weathering test.
Which one is easier to mold?
ABS is the easiest, PC/ABS is intermediate, and PC is the most demanding. If your tool was designed for ABS, running PC/ABS is usually feasible with parameter changes; running PC may require gating and cooling modifications.
Can PC/ABS be electroplated?
Not with standard grades. Plating requires the high-butadiene formulation used in plating-grade ABS. If you need a chrome finish, use ABS.
Which has better chemical resistance?
ABS and PC/ABS are broadly similar and both are vulnerable to solvents, fuels, and aggressive cleaners. PC is slightly worse (more prone to environmental stress cracking). If chemical resistance is the driver, look at PC/PBT instead.
8. Sustainability and End-of-Life
All three materials are thermoplastics and mechanically recyclable, but their end-of-life economics differ.
| Factor | ABS | PC/ABS | PC |
| Recyclability | Good | Moderate | Moderate |
| Sorting difficulty | Low (widely labeled) | Higher (blend) | Low |
| Recycled grade availability | High | Growing | Moderate |
| Impact retention after recycling | Good | −20 to −30% | −20 to −40% |
| Energy recovery value | Good | Good | Good |
PC/ABS is the hardest of the three to recycle because it is a blend — a mixed stream of PC/ABS, ABS, and PC cannot be separated by density or optical sorting alone, and an unseparated stream produces inconsistent mechanical properties. This is a real constraint on closed-loop recycling programs.
Practical guidance: for parts likely to enter a take-back stream, mark the material clearly (ISO 11469 marking: >PC+ABS<), keep regrind in-house, and specify recycled content only after qualifying the actual impact strength of the recycled grade — not the nominal percentage.
9. Total Cost of Ownership: A Worked Example
Consider an enclosure produced at 500,000 units per year, part weight 180 g.
| Cost Element | ABS | PC/ABS | PC |
| Material cost per part (indexed) | 1.00 | 1.28 | 1.70 |
| Scrap rate | 3% | 5% | 9% |
| Cycle time index | 1.00 | 1.12 | 1.28 |
| Tool modification required | — | Minor | Significant |
| Field failure rate (drop-related) | Higher | Low | Low |
| Warranty cost index | 1.00 | 0.45 | 0.40 |
The pellet-price gap between ABS and PC/ABS is real, but it is only one line. ABS’s lower material cost is offset by a higher field-failure rate on any part that sees impact; PC’s superior properties are offset by higher scrap and slower cycles. For this enclosure, PC/ABS lands at the lowest total cost — which is precisely why it dominates the segment.
Set up your own comparison by writing the four numbers that matter: impact requirement, service temperature, cycle time, and field-failure cost. If the field-failure cost is high (safety, warranty, brand), the material with the higher pellet price is usually the cheaper material overall.
10. Next Steps
The right choice is a function of three requirements, not a material preference: impact, service temperature, and whether the part must be clear. Get those three numbers on paper before you open a sample request — it will save you a tooling cycle.
We supply ABS, PC, and PC/ABS in the full grade range from our own compounding facility — general-purpose, high-flow, flame-retardant (UL94 V-0), low-odor automotive, glass-filled, and custom alloys with the PC:ABS ratio tuned to your drop and heat requirements.
What we can send you:
- Full TDS with ratio and DSC verification for every PC/ABS grade
- COA and batch traceability
- UL yellow card copies for FR grades
- Free samples for side-by-side evaluation
[Request TDS and Samples →] | [Ask for an Equivalent Grade Quote →]
Related Reading
- PC/ABS Blend: The Complete Guide to Properties, Grades and Applications
- PC/ABS Ratio Explained: How the PC:ABS Blend Ratio Changes Performance
- PC/ABS Processing Guide: Drying, Melt Temperature and Mold Design
- PC vs PMMA (Acrylic): Optical Clarity, Impact and Cost
- PC/PBT Alloy: Properties, Chemical Resistance and Applications