PC grade selection starts from the process, not the property table.
Injection grades split into general-purpose, optical, medical, and flame-retardant families. Extrusion grades are a distinct family with higher melt viscosity for sheet, profile, and tube — they are not interchangeable with injection grades.
Within each family, the decisions are molecular weight (flow versus toughness), additive package (UV, mold release, FR), and compliance (medical, food, optical).
Finally, remember that PC has poor chemical resistance — no grade of polycarbonate is suitable for fuel, oil, ketone, or chlorinated-solvent contact, and this single limitation eliminates PC from more applications than any other factor.
This guide maps the PC grade space, explains what each family is for, and gives the selection logic and verification points.
1. The Two Structural Divisions
PC grades divide first by process and then by application family. Getting the first division wrong is a common and expensive error.
| Division | Melt Viscosity | Purpose | Typical Products |
| Injection grades | Lower | Fill molds, fast cycles | Enclosures, lenses, housings |
| Extrusion grades | Higher | Hold shape after die | Sheet, film, profile, tube, rod |
Why they are not interchangeable. Extrusion requires melt strength: the extruded sheet or profile must hold its shape after leaving the die, under its own weight, until it cools. That requires a higher molecular weight and higher melt viscosity than injection. If you run an injection grade in extrusion, the melt sags and the sheet thickness varies. If you run an extrusion grade in injection, the melt is too viscous to fill thin walls and cycle times become uneconomic. The two families exist because the requirements are genuinely opposed.
Note the naming trap. A “general-purpose” PC grade is almost always an injection grade. If you need sheet or profile, specify extrusion explicitly — do not assume that a grade chosen for mechanical properties will process in extrusion.
| Process | MFR (300 °C / 1.2 kg) | Molecular Weight |
| Injection, thin wall | 15–25 | Lower |
| Injection, general | 6–12 | Medium |
| Injection, thick wall / high impact | 3–6 | Higher |
| Extrusion, sheet and profile | 2–4 | High |
| Blow molding | 1.5–3 | Highest |
2. Injection Grade Families
2.1 General-Purpose Injection PC
The baseline: transparent, high impact, good heat resistance, easy to process. Used for enclosures, machine guards, light covers, and general transparent parts where no specific optical, medical, or flammability requirement applies.
| Property | Typical Value | Standard |
| Density | 1.20 g/cm³ | ISO 1183 |
| Tensile strength | 60–70 MPa | ISO 527 |
| Tensile modulus | 2,300–2,400 MPa | ISO 527 |
| Notched Izod, 23 °C | 60–90 kJ/m² | ISO 180 |
| HDT at 1.8 MPa | 125–135 °C | ISO 75-2 |
| Light transmission (3 mm) | 87–89% | ASTM D1003 |
| Refractive index | 1.585 | — |
2.2 Optical Grade PC
For lenses, light guides, diffusers, and optical components. The difference from general-purpose is not the polymer — it is the purity and the consistency.
| Requirement | Optical Grade Standard | Why |
| Light transmission | ≥89% at 3 mm | Aesthetic and functional |
| Haze | ≤0.5% | Clarity |
| Birefringence | Controlled | Optical distortion |
| Contamination | Extremely low | Any speck is visible |
| Color consistency | Tight | Batch-to-batch matching |
| Mold release | Often none | Interferes with optics |
| Grade consistency | Batch-certified | Optical design is fixed |
Optical grade is a cleanliness specification as much as a property specification. A single black speck in a lens that is 40 mm across and viewed under magnification is a reject. This is why optical grades carry strict handling requirements, why they usually omit mold release agents, and why they are processed in controlled environments. If you need optical performance but process in a general molding shop, expect a yield problem that has nothing to do with the resin.
Birefringence matters for anything that bends light. PC is inherently birefringent, meaning its refractive index varies with molecular orientation. For a simple light cover this is irrelevant; for a lens or an optical element it causes distortion. Low-birefringence grades exist and are specified for optical elements where wavefront quality matters.
2.3 Medical Grade PC
For device housings, connectors, and components requiring biocompatibility documentation.
| Requirement | Standard | Notes |
| Biocompatibility | USP Class VI, ISO 10993 | Covers the resin as supplied |
| Formulation control | Restricted additives | Colorants and release agents |
| Change control | Notification agreement | Critical for regulatory |
| Sterilization compatibility | Gamma, EtO | Autoclave is limited — see below |
| Traceability | Lot-level | Required for device files |
The autoclave limitation is the key constraint on medical PC. PC hydrolyzes under steam sterilization — the carbonate linkage is vulnerable to hot water — and repeated 134 °C autoclaving causes crazing, yellowing, and impact loss. Medical PC is therefore well suited to gamma and EtO sterilization and poorly suited to autoclave sterilization. If the device must be repeatedly autoclaved, PC is the wrong family; use PEI, PPSU, or PEEK.
The colorant issue recurs. Medical PC with a colored housing requires the colorant to be part of the qualified formulation and covered by the biocompatibility file. A colorant added at the molder’s discretion invalidates the qualification even though the base resin is unchanged.
2.4 Flame-Retardant PC
For electrical and electronic applications requiring UL94 ratings.
| Flame System | Rating | Clarity | Notes |
| Sulfonate-based (KSS) | V-0 to V-2 | Transparent | Low loading, retains clarity |
| Phosphorus-based | V-0 | Translucent | Common for E&E |
| Brominated | V-0 | Opaque | Declining in use |
| Silicone-based | V-0 | Opaque | Good for some applications |
| No FR (inherent) | V-2 at thick sections | Transparent | PC has some inherent FR |
Transparent FR PC usually uses a sulfonate system. Sulfonate flame retardants work at very low loading, which is why they can achieve V-0 while preserving transparency. Phosphorus-based systems are common for opaque E&E parts. Brominated systems are still used but face increasing regulatory pressure and customer restrictions, particularly in Europe.
FR grades change processing. Flame retardants typically reduce melt stability and can increase the tendency to degrade if residence time is excessive. They also frequently require tighter drying and lower melt temperatures than the base resin. Never assume the FR version of a grade processes identically to the unfilled one.
| Grade Type | UL94 at 1.5 mm | Clarity | Typical Use |
| General purpose | V-2 | Transparent | Housings, non-electrical |
| Transparent FR | V-0 | Transparent | Displays, covers |
| Opaque FR | V-0 | Opaque | E&E enclosures, power supplies |
| FR + GF | V-0 | Opaque | Structural E&E, high stiffness |
3. Extrusion Grades Families
Extrusion PC is a distinct family with higher molecular weight, and the grade must match the process.
| Extrusion Product | Grade Requirement | Notes |
| Solid sheet | High MW, high melt strength | Optical sheet needs optical-grade base |
| Multiwall sheet | High MW, good flow for ribs | Balance melt strength and rib filling |
| Film | Very high MW or specific grade | Thin gauge, tight tolerance |
| Profile | High MW, low sag | Complex profiles need melt strength |
| Tube / pipe | High MW | Pressure applications need validation |
| Rod | High MW | Machining stock |
Processing differences that matter:
| Parameter | Injection | Extrusion |
| Drying | 120 °C, 3–4 h | 120 °C, 4–6 h (longer) |
| Melt temperature | 280–310 °C | 260–290 °C |
| Die / mold temperature | 80–100 °C | 90–120 °C (polished rolls) |
| Moisture target | ≤0.02% | ≤0.02% |
| Regrind | 10–20% typical | More restricted for optical sheet |
Sheet polishing temperature controls optical quality. For optical sheet, the roll temperature and surface finish determine haze and surface defects. This is a process control issue rather than a resin issue, but it means the same extrusion grade can produce excellent or unacceptable sheet depending on the line settings.
4. Choosing Molecular Weight: The Flow–Toughness Trade
Across all PC families, molecular weight is the second selection axis after family.
| Molecular Weight | MFR | Flow | Impact | Use |
| Lower | 15–25 | High / Excellent | Lower | Thin wall, long flow, intricate detail |
| Medium | 6–12 | Good | Good | General purpose |
| Higher | 3–6 | Moderate | Higher | Thick wall, high impact |
| Highest | 1.5–3 | Low | Highest | Extrusion, blow molding |
The rule is that low MFR means high impact and poor flow, and high MFR means the opposite. There is no grade that maximizes both. Select on whichever requirement is harder to meet: if the part cannot be filled, flow governs; if the part must survive impact, toughness governs and the tool must be designed to handle the stiffer melt.
| Part Characteristic | MFR Guideline |
| Wall under 1.5 mm, long flow | 15–25 |
| Wall 2–3 mm, general | 6–12 |
| Wall over 4 mm | 3–6 |
| Thick section, impact critical | 3–6 |
| Optical lens, thin | 10–20 (optical grade) |
| Sheet, profile | 2–4 (extrusion) |
5. Additives and Their Consequences
Every additive that solves one problem creates another.
| Additive | Purpose | Consequence |
| UV stabilizer | Outdoor durability | Slight color shift; cost |
| Mold release | Easier ejection | Interferes with optical, bonding, painting |
| Heat stabilizer | Processing stability | Generally benign |
| Flame retardant | UL94 rating | Reduces clarity and color options |
| Antistatic | Static dissipation | May affect optical and bonding |
| Colorant | Appearance | Must match compliance requirements |
| IR absorber | Heat management | Specialized |
Mold release is the additive that causes the most trouble. It reduces surface energy, which improves ejection but degrades paint adhesion, printing, laser marking, and ultrasonic welding. For any part that will be decorated, bonded, or welded, specify a grade without mold release and manage ejection through tool design.
UV stabilization and optical performance are in tension. UV absorbers are themselves colored to some degree, so a UV-stabilized PC is not the same as an optical-grade PC. If you need both outdoor durability and optical clarity, that is a specialized grade and must be specified explicitly.
6. Selection Procedure
Step 1 — Injection or extrusion?
- Sheet, profile, tube, film, rod → extrusion grade.
- Molded part → injection grade.
Step 2 — Any compliance requirement?
- Medical device → medical grade with biocompatibility documentation.
- Electrical/electronic with a flammability requirement → FR grade.
- Food contact → check the food-contact listing; not all PC grades qualify.
- None → continue.
Step 3 — Is optical performance required?
- Yes → optical grade. Confirm transmission, haze, and birefringence requirements, and plan for contamination control in molding.
- No → general purpose.
Step 4 — What is the flow requirement?
- Thin wall or long flow → higher MFR grade.
- Thick wall or impact critical → lower MFR grade.
Step 5 — Will the part be decorated, bonded, or welded?
- Yes → specify no mold release.
- No → standard grade with mold release is fine.
Step 6 — Outdoor exposure?
- Yes → UV-stabilized grade; confirm whether optical performance is also required (and if so, that the combination exists).
| Application | Grade |
| Machine guard, indoor, transparent | General purpose |
| Automotive lens cover, outdoor | Optical grade, UV stabilized |
| Medical device housing, gamma sterilized | Medical grade |
| Power supply enclosure | Opaque FR, V-0 |
| Display cover, transparent, V-0 | Transparent FR |
| Solid sheet for glazing | Extrusion, high MW |
| Light guide | Optical grade, low birefringence |
| Multiwall sheet for roofing | Extrusion, UV stabilized |
7. Frequently Asked Questions
Can I use an injection grade for extrusion?
Generally no. Extrusion requires melt strength to hold shape after the die, which means higher molecular weight and higher melt viscosity than injection grades. An injection grade used in extrusion sags and produces inconsistent thickness.
What is the difference between optical and general-purpose PC?
The base polymer is the same; optical grades are specified for purity, consistency, and low haze, and they typically omit mold release agents. Optical grade is a cleanliness and consistency specification as much as a property specification.
Can PC be autoclaved?
Not repeatedly. PC hydrolyzes under steam sterilization, causing crazing, yellowing, and impact loss. Medical PC is suited to gamma and EtO sterilization. For repeated autoclaving, use PEI, PPSU, or PEEK.
Which PC grades are flame retardant?
FR grades use sulfonate, phosphorus, brominated, or silicone systems to achieve UL94 V-0 or V-2. Sulfonate systems can be transparent; most others are opaque. Confirm the rating at your specific wall thickness — UL94 ratings are thickness-dependent.
Does PC grade affect UV resistance?
Yes. Unstabilized PC yellows and embrittles outdoors, and a UV-stabilized grade is required for any outdoor exposure beyond short term. Note that UV stabilization and optical clarity are in tension, so a grade providing both is specialized.
What MFR do I need for a thin-wall part?
Typically 15–25 g/10 min (300 °C / 1.2 kg) for walls under 1.5 mm with a long flow path. Higher MFR improves fill but reduces impact strength, so confirm that the part still meets its impact requirement.
What is the difference between medical grade and food grade PC?
They are different regulatory frameworks. Medical grades are tested to USP Class VI and ISO 10993 for biocompatibility; food grades must be listed for food contact under FDA 21 CFR or EU 10/2011. A medical grade is not automatically a food grade, and vice versa.
Does mold release affect painting or bonding?
Yes, substantially. Mold release reduces surface energy and degrades paint adhesion, printing, laser marking, ultrasonic welding, and adhesive bonding. For decorated or assembled parts, specify a grade without mold release.
How should I dry PC before processing?
At 120 °C for 3–4 hours (injection) or 4–6 hours (extrusion) in a desiccant dryer, to ≤0.02% moisture. PC hydrolyzes in the melt, and moisture causes splay, silver streaks, and permanent molecular-weight loss.
Can PC be used in contact with fuel or oil? No. PC has poor chemical resistance to fuels, oils, ketones, esters, and chlorinated solvents — it stress-cracks and can dissolve. No grade of polycarbonate is suitable for these media. Use PC/PBT, PBT, or PA instead.
What is the light transmission of optical PC?
Typically 87–89% at 3 mm, with haze below 0.5% for optical grades. PMMA achieves slightly higher transmission (92%), which is one reason it is preferred for some optical applications despite its lower impact strength.
What is the difference between glass-filled and unfilled PC?
Glass-filled PC (typically GF10–GF30) raises stiffness, lowers coefficient of thermal expansion, and reduces creep, but it becomes opaque and more notch-sensitive — elongation at break falls sharply. Use it for structural parts, not for anything needing transparency or impact at a sharp corner.
How does PC compare with PC/ABS for an enclosure?
PC offers better transparency and slightly better heat resistance; PC/ABS offers better flow, lower cost, better chemical resistance in some media, and easier processing. For a cosmetic opaque enclosure, PC/ABS is usually the better choice; for a transparent or higher-heat application, PC is.
Can PC be laser marked or printed?
Yes, but mold release interferes with both. Specify a no-mold-release grade for any part that will be laser marked, pad printed, or hot stamped, and verify adhesion with your specific marking system.
Why does my PC part have a yellow tint after processing?
Usually excessive melt temperature or residence time, which degrades the polymer and yellows it. PC is sensitive to thermal history; reduce melt temperature, shorten residence time, and verify the dryer is working. Note that a properly processed PC is slightly warm in tone by nature — evaluate against a reference sample, not absolute expectation.
Is PC recyclable?
PC is recyclable (code 7 for “other”), and industrial regrind is routinely reused at 10–20% in non-critical parts. Post-consumer PC recycling exists but is less developed than for HDPE or PET. Regrind reduces optical quality and is generally avoided in optical and medical applications.
8. Next Steps
The pc grade selection sequence is: process first (injection or extrusion), compliance second (medical, FR, food), optical third, then flow versus toughness, then additives. And always check the chemical environment — no grade of PC survives fuel, oil, or solvent contact, and that limitation overrides every other consideration.
We supply PC in general-purpose, optical, medical, flame-retardant, UV-stabilized, extrusion, and glass-filled grades, with full documentation for medical, food-contact, and E&E applications.
What we can send you:
- Grade range overview with property data
- Optical grade transmission and haze data
- Medical grade biocompatibility documentation
- UL yellow cards for FR grades
- Food-contact listings where applicable
- Samples for your own testing
[Request the PC Grade Selector →] | [Ask for a Grade Recommendation →]
Related Reading
- PC vs PMMA (Acrylic): Optical Clarity, Impact and Cost
- PC/ABS Blend: The Complete Guide to Properties, Grades and Applications
- PC/ABS Alloy: Properties, Applications and Injection Molding
- Flame-Retardant PC/ABS: UL94 V-0 Grades for IT and EV Housings
- PC/PBT Alloy: Properties, Chemical Resistance and Applications