Polycarbonate (pc) resin is the only commodity-priced engineering plastic that delivers high impact strength, optical clarity, heat resistance to about 130 °C, and inherent flame retardancy in the same material — and that combination is why it holds positions in electrical enclosures, automotive lighting, medical devices, and safety glazing that no other polymer has displaced.
The trade-offs are equally specific: PC is notch sensitive, it stress-cracks in common solvents including alcohol and many cleaning agents, it hydrolyses if processed wet, and it yellows under UV unless stabilized. Every serious PC failure in the field traces back to one of those four.
Selection therefore starts not with a property table but with four questions: what impact does the part face, what chemicals will touch it, how will it be dried and molded, and how long will it be outdoors.
1. What Polycarbonate Is
Polycarbonate is an amorphous thermoplastic built from bisphenol-A (BPA) and a carbonate linkage. Two industrial routes exist:
- Interfacial phosgene process — BPA in aqueous alkaline solution reacts with phosgene in an organic phase. This is the historical route and still dominant for high-clarity grades.
- Melt transesterification process — BPA reacts with diphenyl carbonate in the melt, with phenol as a by-product. This route avoids phosgene and is increasingly used for new capacity.
The chemistry matters commercially for two reasons. First, residual monomer and catalyst residues control optical quality — optical and medical grades are defined as much by what has been removed as by what is present. Second, the carbonate bond is hydrolytically unstable at melt temperature, which is the origin of PC’s demanding drying requirement.
The aromatic backbone gives PC its stiffness and its high glass transition (Tg ≈ 145–150 °C). The carbonate linkage gives it chain flexibility and impact toughness. The result is a polymer that is simultaneously rigid and ductile — an unusual combination that most plastics achieve only by adding rubber, which costs heat resistance and clarity.
2. Property of Polycarbonate
| Property | Typical Value | Unit | Test Standard |
| Density | 1.20 | g/cm³ | ISO 1183 |
| Glass transition (Tg) | 145–150 | °C | ISO 11357 (DSC) |
| Tensile strength at yield | 60–70 | MPa | ISO 527 |
| Tensile modulus | 2,300–2,400 | MPa | ISO 527 |
| Elongation at break | 90–130 | % | ISO 527 |
| Flexural modulus | 2,300–2,400 | MPa | ISO 178 |
| Notched Izod, 23 °C | 65–90 | kJ/m² | ISO 180 |
| Notched Izod, −30 °C | 12–20 | kJ/m² | ISO 180 |
| Charpy unnotched, 23 °C | No break | — | ISO 179 |
| HDT at 1.82 MPa | 125–135 | °C | ISO 75 |
| HDT at 0.45 MPa | 135–143 | °C | ISO 75 |
| Vicat softening (B50) | 145–150 | °C | ISO 306 |
| Light transmission (3 mm) | 88–90 | % | ISO 13468 |
| Haze (3 mm) | < 1 | % | ISO 14782 |
| Refractive index | 1.584 | — | ISO 489 |
| Limiting oxygen index | 25–27 | % | ISO 4589 |
| UL94 rating (unmodified) | V-2 at 1.5 mm | — | IEC 60695-11-10 |
| Water absorption, 24 h | 0.15–0.35 | % | ISO 62 |
| Coefficient of linear expansion | 6.5–7.0 × 10⁻⁵ | 1/K | ISO 11359 |
| Thermal conductivity | 0.20 | W/m·K | ISO 22007 |
| Dielectric constant (1 MHz) | 2.9–3.0 | — | IEC 60250 |
| Volume resistivity | > 10¹⁵ | Ω·cm | IEC 62631 |
| Comparative tracking index | 250–600 | V | IEC 60112 |
Four entries in that table are worth highlighting because they explain where PC wins and loses.
Notched impact of 65–90 kJ/m² is extraordinary — roughly 20–40 times PMMA or PS, and several times most engineering plastics. It is the property that made PC the material of choice for safety helmets, machine guards, and power tool housings.
HDT of 125–135 °C at 1.82 MPa is the highest among transparent plastics by a wide margin. PMMA softens around 100 °C, PS around 85 °C, and PET around 75 °C. This is why PC owns automotive lighting and hot-appliance parts.
Light transmission of 88–90% with haze below 1% puts PC close to PMMA optically while being far tougher. The gap is small enough that PC often substitutes for acrylic where impact matters.
CTI of 250–600 V is a wide range because it is formulation-dependent, and it is one of the most frequently under-specified properties in electrical design. Two PC grades that look identical in a data sheet can differ by more than a factor of two in tracking resistance.
3. The Four Failure Modes
Almost every PC field failure belongs to one of four categories. Understanding them is more useful than memorizing the property table.
3.1 Notch sensitivity
PC’s notched impact is high, but its ratio of notched to unnotched impact is low — roughly 1:20. A sharp feature, a scratch, a machining mark, or a molded-in stress concentration converts a tough material into a brittle one.
| Feature | Stress Concentration Factor | Practical Rule |
| Sharp internal corner | 3–5 | Radius ≥ 0.5× wall thickness |
| Scratch or tool mark | 2–4 | Avoid in high-stress zones |
| Weld line | 2–3 | Move gate; reinforce with ribs |
| Gate area | 2–4 | Enlarge gate, reduce packing |
| Press fit | 3–6 | Interference ≤ 0.3% |
This is why the same PC that survives a hammer blow can crack when a screw is driven into a molded hole without clearance.
3.2 Environmental stress cracking
PC is attacked by a surprisingly long list of everyday chemicals, and attack requires both the chemical and a tensile stress. Remove either and the part survives.
| Agent | Effect on Stressed PC |
| Isopropyl alcohol | Severe crazing |
| Ethanol | Moderate to severe |
| Acetone, MEK | Immediate attack |
| Toluene, xylene | Severe |
| Ammonia cleaners | Severe |
| Chlorinated solvents | Severe |
| Iodine / povidone-iodine | Severe |
| Concentrated alkalis | Hydrolysis plus cracking |
| Hot water (long exposure) | Hydrolysis |
| Dilute acids | Generally good |
| Silicone oil, mineral oil | Good |
The practical consequence is that cleaning protocols are part of the material specification. A PC housing specified without reference to the disinfectant used in the field is an incomplete specification.
3.3 Hydrolytic degradation
At melt temperature, water attacks the carbonate bond and cuts the chain. The damage is invisible in the short term and appears as brittleness weeks later. PC must be dried to below 0.02% moisture before processing, which requires a desiccant dryer at 120 °C with a dew point of −20 °C or lower. Hot-air ovens do not achieve this.
3.4 UV yellowing
PC absorbs UV and generates colour bodies through photo-Fries rearrangement. Unstabilized PC yellows visibly within 1,000–2,000 hours of outdoor exposure and embrittles at the surface. Stabilized grades extend this substantially, and co-extruded UV cap layers extend it further.
4. The PC Resin Grade Landscape
PC is sold across a set of functional families. Within each family, the primary variable is melt volume rate (MVR), measured at 300 °C/1.2 kg per ISO 1133, which is the inverse of molecular weight.
| MVR (cm³/10 min) | Flow | Toughness | Typical Use |
| 3–6 | Very low | Highest | Extrusion, sheet, thick sections |
| 6–10 | Low | High | Thick-wall injection, structural |
| 10–16 | Medium | Good | General injection molding |
| 16–25 | Medium-high | Moderate | Thin-wall, long flow |
| 25–40 | High | Lower | Very thin wall, fast cycles |
| PC Grades Family | What It Adds | Typical Application |
| General purpose PC | Nothing — the baseline | Housings, brackets, general parts |
| High flow PC | Lower molecular weight | Thin-wall, complex flow |
| Extrusion / sheet PC | Melt strength, UV options | Glazing, signage, machine guards |
| Flame retardant PC | V-0 at 1.5–3.0 mm | E&E enclosures, chargers |
| UV-stabilized PC | HALS + UV absorber | Outdoor parts, automotive exterior |
| Optical PC | Low haze, low birefringence | Lenses, light guides, displays |
| Medical PC | Low extractables, documented | Devices, fluid paths, housings |
| Food contact PC | Compliant additives | Food processing, packaging |
| Wear / lubricated PC | PTFE, silicone | Gears, bearings, sliding parts |
| Glass-filled PC | 10–40% glass | Stiffness, low CLTE, creep |
| High heat PC | Copolycarbonate, Tg > 160 °C | Automotive under-hood, lighting |
Two structural notes. Glass-filled PC is a different material in practice — it gains stiffness and dimensional stability but loses most of its impact strength and its transparency, so it does not belong in the same conversation as unfilled PC. High-heat copolycarbonates (sold under separate brand names) are a different chemistry with a Tg above 160 °C; they are the answer when standard PC runs out of thermal margin.
5. Processing
5.1 Drying — the non-negotiable step
| Parameter | Value |
| Temperature | 120 °C |
| Time | 3–4 hours (up to 6 h for thick regrind) |
| Dew point | ≤ −20 °C |
| Target moisture | < 0.02% |
| Dryer type | Desiccant, not hot air |
A hot-air oven at 120 °C will remove surface moisture and leave the interior wet. The result is splay, silver streaks, and a molecular weight drop that shows up as brittle parts months later.
5.2 Injection molding
| Parameter | Typical Range | Notes |
| Melt temperature | 280–320 °C | Lower for high MVR |
| Mold temperature | 80–110 °C | Higher improves surface, reduces stress |
| Injection speed | Moderate to fast | Fast for thin wall |
| Holding pressure | 50–80% of injection | Avoid over-packing at gate |
| Back pressure | Low | High back pressure adds shear history |
| Screw speed | Moderate | Keep residence time short |
| Regrind | 15–20% | Re-dry; requalify UL if listed |
High mold temperature is the single most effective way to reduce molded-in stress. A part molded at 60 °C and one molded at 100 °C from the same material will behave differently in a solvent test.
5.3 Extrusion
PC sheet and profile extrusion requires low MVR for melt strength, melt temperatures of 260–300 °C, and a polished cooling stack for optical quality. Drying is the same requirement as injection. Sheet thickness tolerance and residual stress are controlled by the cooling rate — fast cooling freezes in stress that later causes thermoforming problems.
5.4 Annealing
Where stress relief is required, anneal at 120–125 °C for one hour per millimetre of wall plus one hour, and cool at 10–15 °C per hour. Fast cooling recreates the thermal gradient that caused the stress. Expect 0.1–0.5% shrinkage, and design the tool allowance accordingly.
5.5 Secondary operations
PC machines well but is notch sensitive, so use sharp tooling, avoid scratching, and relieve stress before and after rough machining. Solvent bonding works with dichloromethane or cyclohexanone but creates stress concentrations at the joint. Ultrasonic welding works well with a proper joint design. Painting requires a compatible primer — many solvents attack PC.
6. Design Rules That Prevent Most Failures
PC’s failure modes are predictable, and six design decisions address almost all of them. They cost little at the drawing stage and are expensive to retrofit.
| Design Decision | Rule of Thumb | Failure It Prevents |
| Wall uniformity | Variation < 25% of nominal; gradual transitions | Sink, warpage, differential cooling stress |
| Internal radii | ≥ 0.5× wall, preferably 1× | Notch-initiated cracking at corners |
| Boss design | Wall 0.6× nominal; radius at base; 0.3% max interference for press fits | Boss cracking, hoop stress |
| Rib proportions | Thickness 0.5–0.6× wall; depth ≤ 3× wall | Sink marks, void formation |
| Gate sizing | Gate depth ≥ 0.6× wall; avoid small gates on thick sections | Frozen-in shear stress, gate blush |
| Draft and ejection | 1–2° draft; ejector area adequate | Scuffing, ejection stress, warpage |
Two of these deserve emphasis because they cause the majority of field failures.
Boss design. A boss is a cylinder with a hole, and it concentrates stress at its base while the surrounding material shrinks around it. A boss with wall thickness equal to the nominal wall creates a thick section that cools last, pulls the surrounding material, and leaves a ring of tensile stress — exactly where a screw will later add more. Boss wall at 0.6× nominal, a generous base radius, and gussets where space allows.
Press fits. Interference generates hoop stress proportional to the interference divided by the diameter. For PC, keep interference below 0.3% of diameter, and prefer a design that uses a retaining feature rather than pure friction. A 1% interference fit in PC will often crack within days — sometimes within hours if the part is also exposed to a solvent.
A useful discipline is to treat every sharp corner on a PC drawing as a defect to be justified, not a default. In practice, adding radii and reducing wall variation fixes more PC field failures than changing grade, and it costs nothing.
7. Applications by Industry
| Industry | Typical Parts | Why PC |
| Electrical and electronics | Enclosures, chargers, connectors, switchgear | Impact + V-0 + CTI + dimensional stability |
| Automotive | Headlamp lenses, interior trim, grilles, EV battery parts | Heat + clarity + impact |
| Medical | Device housings, fluid paths, oxygenators, syringe barrels | Clarity + toughness + sterilizability (gamma, EtO) |
| Construction | Glazing, roofing, sound barriers, safety guards | Impact + clarity + light weight |
| Consumer | Luggage, helmets, bottles, appliances | Impact + appearance |
| Industrial | Machine guards, tool housings, light covers | Impact + transparency |
| Lighting | LED lenses, diffusers, light guides | Optical quality + heat |
| EV and energy | Charging housings, battery covers, busbar supports | FR + CTI + thermal cycling |
Two of these are growing fastest. EV charging and battery components combine flammability, tracking, and thermal-cycling requirements that PC meets better than most alternatives. LED lighting needs optical clarity at temperatures that rule out PMMA and PS.
8. PC Against the Alternatives
| Property | PC | PMMA | PS | PC/ABS | PET | PA66 |
| Notched Izod (kJ/m²) | 65–90 | 1.5–2 | 2–3 | 35–50 | 4–6 | 5–8 |
| HDT at 1.82 MPa (°C) | 125–135 | 85–100 | 75–85 | 95–110 | 70–80 | 240–250 |
| Light transmission (%) | 88–90 | 92 | 88–90 | Opaque | 85–90 | Opaque |
| Haze (%) | < 1 | < 0.5 | 2–4 | — | 1–3 | — |
| Inherent FR | V-2 at 1.5 mm | Burns | Burns | V-2 at 3 mm | V-2 | V-2 |
| Chemical resistance | Poor–fair | Good | Poor | Fair | Good | Good |
| UV resistance | Fair (stabilized) | Excellent | Poor | Fair | Good | Fair |
| Cost index | 100 | 70–85 | 55–65 | 75–85 | 65–75 | 90–105 |
The pattern is consistent: PC wins on impact plus heat plus clarity, and loses on chemical resistance and UV. PMMA is clearer and cheaper but brittle and heat-limited. PS is cheaper still and even more brittle. PC/ABS trades heat and clarity for cost and processability. PET is chemically tougher but thermally weaker. PA66 is far hotter but opaque and moisture sensitive.
That is why PC has never been displaced from its core applications despite being more expensive than every alternative except the high-temperature nylons.
9. Selection Procedure
A reliable sequence, in order:
Step 1 — Define the impact requirement. Not “tough” but a number: drop height and mass, or notched Izod at a stated temperature. Cold impact is the usual failure, so specify at −20 or −30 °C.
Step 2 — Define the thermal requirement. Continuous service temperature and peak excursion. If the peak exceeds 130 °C, standard PC is out and a high-heat copolycarbonate or a different polymer is required.
Step 3 — List every chemical the part will contact. Including cleaning agents, disinfectants, adhesives, paints, and lubricants. This step eliminates more PC applications than any other.
Step 4 — Define the optical requirement. Transmission, haze, and colour at the actual wall thickness — not at 3 mm on a data sheet.
Step 5 — Define the compliance requirement. UL94 thickness and colour, CTI, glow wire, food contact, medical documentation, automotive OEM specification. Compliance is grade-specific and often colour-specific.
Step 6 — Choose the MVR band from the process and wall thickness. Extrusion 3–6, general injection 10–16, thin wall 20–35.
Step 7 — Verify with a trial in the real tool, and test aged parts, not just fresh ones.
10. Incoming Inspection
| Check | Method | What It Reveals |
| MVR | ISO 1133 at 300 °C/1.2 kg | Molecular weight, grade identity |
| Density | ISO 1183 | Filled vs unfilled, contamination |
| Moisture | Karl Fischer | Drying adequacy |
| FTIR | ATR | PC vs PC/ABS vs other polymers |
| Colour | Lab* on molded chip | Grade family, lot consistency |
| Ash | TGA or furnace | Filler content |
| UL Yellow Card | UL Product iQ by file number | Whether grade, colour, thickness are listed |
| COA traceability | Lot number | Whether the material is what the label says |
FTIR plus MVR is a five-minute screen that catches most substitutions. The UL file number is the compliance anchor — a certificate image is easy to copy, a database entry is not.
11. Frequently Asked Questions
What is polycarbonate made from?
Bisphenol-A and a carbonate source — either phosgene in the interfacial process or diphenyl carbonate in the melt transesterification process. The aromatic BPA unit gives stiffness and heat resistance; the carbonate linkage gives toughness and flexibility.
Is polycarbonate food safe and BPA-free?
Food-contact PC grades are available and are regulated under FDA 21 CFR and EU 10/2011, with specific migration limits for BPA. “BPA-free” is a marketing term, not a regulatory category — polycarbonate is by definition a BPA-based polymer. For applications where BPA is prohibited, the answer is a different material, not a different PC grade.
Why does polycarbonate crack around screws and inserts?
Notch sensitivity plus molded-in stress. A sharp thread or a press fit with excessive interference creates a stress concentration that exceeds the material’s local strength. Fixes: increase boss diameter, add clearance, use threaded inserts designed for plastics, and anneal before assembly.
Can polycarbonate be used outdoors?
Yes, with a UV-stabilized grade. Unstabilized PC yellows within 1,000–2,000 hours of QUV exposure and embrittles at the surface. Stabilized grades extend service life considerably, and co-extruded UV cap layers extend it further. For long-life outdoor glazing, a cap layer is the standard solution.
What is the maximum service temperature of PC?
About 125–130 °C continuous for standard grades, with HDT at 1.82 MPa of 125–135 °C. High-heat copolycarbonates extend this to 160 °C and above. Above that, the material is no longer PC in any practical sense.
Why must PC be dried before processing?
Because water hydrolyses the carbonate bond at melt temperature, cutting molecular weight. The damage is not visible immediately — it appears as brittleness and reduced impact weeks later. Dry to below 0.02% at 120 °C in a desiccant dryer with a dew point of −20 °C or lower.
What is the difference between PC and PC/ABS?
PC/ABS is a blend that trades heat resistance (HDT 95–110 °C versus 125–135 °C) and transparency for lower cost, better flow, and easier processing. It is the right choice for cosmetic enclosures that do not exceed 100 °C; PC is the right choice when impact plus heat plus clarity are all required.
Can polycarbonate be sterilized?
Gamma and ethylene oxide sterilization are compatible with most PC grades. Steam autoclaving is not — hydrolysis at 121 °C degrades the carbonate bond and parts embrittle over repeated cycles. Some grades are qualified for limited autoclave exposure; confirm for the specific grade and cycle count.
Does polycarbonate yellow during processing?
Yes, if overheated or processed wet. Hydrolysis products and thermal oxidation both create colour bodies. Check the dryer first, then the melt temperature profile and residence time. A well-run process produces minimal yellowing.
What is the CTI of polycarbonate and why does it matter?
250–600 V depending on grade. CTI determines the creepage and clearance distances required in electrical design, so a grade with 250 V may require larger spacing than one with 600 V — which can change the whole enclosure design. Specify it explicitly for EV and industrial applications.
Is polycarbonate recyclable?
Yes, mechanically, with limits — 15–20% regrind in a virgin blend, and less for optical grades. Post-consumer PC recycling is commercially established for water bottles, optical media, and sheet. Chemical recycling back to BPA is also commercial, producing virgin-equivalent resin at a premium.
Why is PC more expensive than PS or ABS?
Because the monomer is more expensive, the polymerization is more demanding, and the properties justify it. PC typically trades at 1.5–2× the price of ABS and 2× the price of PS. The premium is recovered in applications where impact, heat, and clarity are all required — where the alternatives simply do not work.
Can PC be transparent and flame retardant at the same time?
Yes. Transparent FR PC grades use sulfonate chemistry and achieve V-0 at 1.5–3.0 mm with 85–89% transmission and low haze. They cost significantly more than opaque FR grades, and the optical properties are thickness-dependent.
What is the difference between PC and PMMA for optical parts?
PMMA is clearer (92% versus 88–90%), harder, and more UV stable, and it costs less. PC is 20–40 times tougher and has a much higher HDT. Choose PMMA for optical quality in a protected environment; choose PC where the part will be impacted or will run hot.
How thick can PC sheet be and still be transparent?
Optical quality degrades with thickness. Standard glazing sheet runs 2–12 mm with good clarity; beyond 12 mm, transmission falls and haze rises measurably. For thick sections, specify optical-grade resin and verify transmission at the actual thickness.
12. Next Steps
Polycarbonate rewards a disciplined selection process because its strengths and weaknesses are both extreme. Get the four questions right — impact, chemicals, drying, UV — and PC will outperform almost anything else in the application. Get one wrong, and the failure will be sudden and often expensive.
We supply PC across general purpose, high-flow, FR, UV-stabilized, optical, medical, food-contact, glass-filled, and extrusion grades, with lot-specific MVR, density, and colour data, UL Yellow Cards for your thickness and colour, and processing support from drying through annealing. Because we compound in-house, we can also develop a custom formulation when no catalogue grade fits — and we will tell you when a different polymer is the better answer.
What we can send you:
- Grade selection table by MVR band and application
- Full property data with test standards
- UL Yellow Cards for your thickness and colour
- Processing sheets — drying, injection, extrusion, annealing
- Chemical resistance data for your cleaning agents
- Optical data at your wall thickness
- Free samples for your own testing
[Request a PC Grade Pack →] | [Ask About PC Selection for Your Part →]
Related Reading
- PC Grade Selection: Optical, Medical, FR and Extrusion Grades
- PC Annealing and Residual Stress: Preventing Crazing in Service
- PC Melting Point and Drying: A Processing Guide
- Why Does Polycarbonate Yellow? Causes and Prevention
- Flame-Retardant PC: UL94 V-0 Grades and Applications
- PC for Medical Devices: Sterilization Compatibility
- PC Sheet and Film: Extrusion, Thermoforming and Secondary Operations
- PC Recycling and rPC: Depolymerization and Mechanical Routes
- PC vs ABS: Which Engineering Plastic for Your Application
- PC vs PMMA (Acrylic): Optical Clarity, Impact and Cost
- PC/ABS Blend: Properties, Grades and Applications
- Covestro Makrolon PC Grades: Optical, Medical and FR