Makrolon 6487 RE PC Resin Flame Retardant
Makrolon 6487 RE is a partially bio-circular polycarbonate resin (PC) with UL 94V-0/1.5mm and 5VA/3.0mm flame retardancy. Its medium viscosity, UV stabilization, easy-release properties, and opaque color options make it ideal for injection-molded safety-critical parts, combining sustainability (ISCC PLUS mass balance) with robust performance.
Plastic Granules
Download PDF
ISO TDS
Typical property data
Physical Properties (Rheological)
- Melt Volume-Flow Rate (MVR): 9.0 cm³/10 min (300 °C/1.2 kg, ISO 1133)
- Melt Mass-Flow Rate (MFR): 10 g/10 min (300 °C/1.2 kg, ISO 1133)
- Molding Shrinkage, Parallel: 0.7% (ISO 294-4)
- Molding Shrinkage, Normal: 0.75% (ISO 294-4)
Mechanical Properties (23 °C/50% r. h.)
- Tensile Modulus: 2450 MPa (1 mm/min, ISO 527-1,-2)
- Yield Stress: 66 MPa (50 mm/min, ISO 527-1,-2)
- Yield Strain: 6.0% (50 mm/min, ISO 527-1,-2)
- Flexural Modulus: 2450 MPa (2 mm/min, ISO 178)
- Flexural Strength: 99 MPa (2 mm/min, ISO 178)
- Charpy Notched Impact Strength (23 °C): 70 kJ/m² (3 mm, ISO 21305/ISO 179/1eA)
- Charpy Notched Impact Strength (-30 °C): 12 kJ/m² (3 mm, ISO 21305/ISO 179/1eA)
Thermal Properties
- Glass Transition Temperature: 141 °C (10 °C/min, ISO 11357-1,-2)
- Temperature of Deflection Under Load (1.80 MPa): 122 °C (ISO 75-1,-2)
- Temperature of Deflection Under Load (0.45 MPa): 134 °C (ISO 75-1,-2)
- Vicat Softening Temperature: 141 °C (50 N, 50 °C/h, ISO 306)
- Coefficient of Linear Thermal Expansion (23-55 °C, Parallel/Normal): 0.65 × 10⁻⁴/K (ISO 11359-1,-2)
- Burning Behavior: UL 94 V-0 (1.5 mm), UL 94 5VA (3.0 mm)
Electrical Properties (23 °C/50% r. h.)
- Relative Permittivity (100 Hz): 3.1 (IEC 60250)
- Relative Permittivity (1 MHz): 3.0 (IEC 60250)
- Dissipation Factor (100 Hz): 0.0008 (IEC 60250)
- Dissipation Factor (1 MHz): 0.009 (IEC 60250)
- Volume Resistivity: 1 × 10¹⁴ Ohm·m (IEC 62631-3-1)
- Surface Resistivity: 1 × 10¹⁶ Ohm (IEC 62631-3-2)
- Electrical Strength: 34 kV/mm (1 mm, IEC 60243-1)
Other Properties (23 °C)
- Water Absorption (Saturation): 0.30% (ISO 62)
- Water Absorption (Equilibrium): 0.12% (23 °C/50% r. h., ISO 62)
- Density: 1200 kg/m³ (ISO 1183-1)
Processing and Drying Conditions
- Injection Molding – Melt Temperature: 280–320 °C (ISO 294)
- Injection Molding – Mold Temperature: 80–120 °C (ISO 294)
- Drying Temperature: 120 °C (Dry Air Dryer Only)
- Drying Time: 2–3 hours
- Moisture Content (Max): ≤ 0.02%
Use & Applications
- Electrical: Circuit breakers, relay housings, EV charging components.
- Automotive: Dashboard switches, sensor housings, lighting enclosures.
- Industrial: Flame-retardant tool housings, safety equipment, machine guards.
- Consumer: Power adapters, smart-home devices requiring opaque, UV-stable parts.
Features & Benefits
Uncompromising Flame Safety
It achieves UL 94V-0 at ultrathin 1.5mm and 5VA at 3.0mm, with high oxygen index (36%). Perfect for electrical housings or automotive components where fire resistance is non-negotiable.
Sustainable & High-Performance
Partially bio-circular via ISCC PLUS mass balance, reducing carbon footprint without sacrificing mechanical strength or UV stability. Ideal for eco-conscious industrial designs.
Easy Processing & Durability
Medium viscosity (MVR 9.0 cm³/10 min) and low molding shrinkage (0.6–0.8%) ensure smooth injection molding, while high impact resistance (>50% strain at break) extends product lifespan.
Makrolon® 6487 RE Related Flame Retardant Grades
Disclaimer: Grades below are potential alternatives for comparison only. Not direct drop-in replacements. Typical values from Covestro ISO TDS; verify UL94 colors/thickness on current UL Yellow Card. RoHS/REACH/halogen/PFAS status not confirmed unless report provided.
| Grade | Positioning | UL94 (ISO TDS) | MVR | HDT (1.80 MPa) | Notched Impact (23°C/3mm) | Color | UV / UL 746C f1 |
|---|---|---|---|---|---|---|---|
| 6487 | Parent grade (fossil); 5VA; UV | V-0 @1.5mm; 5VA @3.0mm | 9.0 cm³/10min | 122°C | Charpy 70P(C); Izod 70P(C) | Opaque | Yes / N/A |
| 6485 | Medium viscosity; 5VA; no UV | V-0 @1.5mm; 5VA @3.0mm | 9.0 cm³/10min | 124°C | Charpy 70P(C); Izod 65P(C) | Opaque | No / N/A |
| 6267 X RE CQ | Bio-circular; low viscosity; UV | V-0 @1.5mm | 19 cm³/10min | 122°C | Charpy 60P(C); Izod 15P(C) | Opaque | Yes / N/A |
| 6555 RE CQ | RE CQ; medium viscosity | V-0 @3.0mm; V-2 @1.0mm | 10 cm³/10min | 125°C | Charpy 70P; Izod 65P | N/A | N/A / N/A |
👉 Full Portfolio: Browse all 27+ grades on the Covestro Flame Retardant PC Resin Hub.