Plastic Granules
LG ABS ER400 Heat Resistant Grade
LG ABS ER400-C is a heat-resistant ABS resin designed for injection molding and extrusion, offering medium heat resistance, low TVOC emissions, low gloss, and excellent extrusion kneading performance. Ideal for general sheet and edge band applications.
Typical property data
Physical Properties
- Specific Gravity: 1.04 (ASTM D792)
- Mold Shrinkage: 0.4–0.8% (ASTM D955)
- Melt Flow Index: 7 g/10min at 220℃, 10kg (ASTM D1238)
Mechanical Properties
- Tensile Strength at Yield: 53 MPa at 23℃, 50mm/min, 3.2mm (ASTM D638)
- Tensile Elongation at Break: Minimum 20% at 23℃, 50mm/min, 3.2mm (ASTM D638)
- Flexural Strength: 90 MPa at 23℃, 15mm/min, 3.2mm (ASTM D790)
- Flexural Modulus: 2580 MPa at 23℃, 15mm/min, 3.2mm (ASTM D790)
- Rockwell Hardness: R-Scale 110 (ASTM D785)
Impact Properties
- Izod Impact Strength Notched (3.2mm): 270 J/m at 23℃ (ASTM D256)
- Izod Impact Strength Notched (6.4mm): 200 J/m at 23℃ (ASTM D256)
Thermal Properties
- Heat Deflection Temperature (HDT): 93℃ at 1.82 MPa, edgewise, 6.4mm, unannealed (ASTM D648)
- Vicat Softening Temperature: 103℃, 50N, 50℃/h (ASTM D1525)
Injection Molding Parameters
- Drying Temperature: 80–90℃, 3–4 hours
- Injection Temperature: 220–290℃
- Mold Temperature: 40–80℃
- Screw Speed: 30–60 rpm
Extrusion Parameters
- Drying Temperature: 80–90℃, 3–4 hours
- Moisture Content: ~0.01%
- Extrusion Temperature: 180–250℃
Features & Benefits
Medium Heat Resistance
With a Heat Deflection Temperature of up to 92°C, ER400-C maintains structural integrity in warm environments, making it suitable for applications like appliance housings and automotive interior parts.
Low TVOC & Eco-Friendly
This material meets strict indoor air quality standards with low VOC emissions, ensuring safer use in consumer products and enclosed spaces without compromising performance.
Low Gloss & Aesthetic Flexibility
The matte finish reduces glare and hides fingerprints, ideal for visible surfaces in electronics, furniture, and decorative trim where a premium, non-reflective look is desired.
Use & Applications
- General Extruded Sheet
- Edge Band for Furniture and Panels