ULTEM™ Resin 1010M Unreinforced Amorphous PEI Resin

ULTEM™ Resin 1010M is an unreinforced amorphous PEI resin with 217°C Tg, high flow, and reduced internal mold release. It delivers strong mechanical, electrical, and dimensional stability at high temperatures, with inherent flame retardancy and RoHS compliance.

Associated Documents

TDS - Global

Typical property data

Physical Properties
  • Density: 1.27 g/cm³ (ISO 1183)
  • Specific Gravity: 1.27 (ASTM D792)
  • Moisture Absorption, 23°C / 50% RH / 24 hrs: 0.2% (ISO 62-4)
  • Moisture Absorption, 23°C / 50% RH / Equilibrium: 0.7% (ISO 62-4)
  • Water Absorption, 23°C / 24 hrs: 0.25% (ISO 62-1)
  • Water Absorption, 23°C / Saturated: 0.25% (ISO 62-1)
  • Water Absorption, 23°C / 24 hrs: 0.25% (ASTM D570)
  • Water Absorption, 23°C / Saturated: 1.25% (ASTM D570)
  • Melt Volume Rate, 360°C / 5.0 kg: 25 cm³/10 min (ISO 1133)
  • Melt Volume Rate, 340°C / 5.0 kg: 13 cm³/10 min (ISO 1133)
  • Melt Flow Rate, 337°C / 6.6 kgf: 17.8 g/10 min (ASTM D1238)
  • Poisson’s Ratio: 0.36 (ASTM E132)
  • Mold Shrinkage, Flow, 3.2 mm: 0.5–0.7% (SABIC Method)
  • Mold Shrinkage, Cross Flow, 3.2 mm: 0.5–0.7% (SABIC Method)
Mechanical Properties
  • Tensile Stress at Yield, 50 mm/min: 110 MPa (ISO 527)
  • Tensile Strain at Yield, 50 mm/min: 6% (ISO 527)
  • Tensile Strain at Break, 50 mm/min: 50% (ISO 527)
  • Tensile Modulus, 1 mm/min: 3200 MPa (ISO 527)
  • Flexural Stress at Yield, 2 mm/min: 160 MPa (ISO 178)
  • Flexural Modulus, 2 mm/min: 3300 MPa (ISO 178)
  • Ball Indentation Hardness, H358/30: 140 MPa (ISO 2039-1)
  • Rockwell Hardness: M106 (ISO 2039-2)
  • Tensile Stress at Yield, Type I, 50 mm/min: 115 MPa (ASTM D638)
  • Tensile Strain at Yield, Type I, 50 mm/min: 7% (ASTM D638)
  • Tensile Strain at Break, Type I, 50 mm/min: 60% (ASTM D638)
  • Tensile Stress at Yield, Type I, 5 mm/min: 110 MPa (ASTM D638)
  • Tensile Strain at Yield, Type I, 5 mm/min: 7% (ASTM D638)
  • Tensile Strain at Break, Type I, 5 mm/min: 60% (ASTM D638)
  • Tensile Modulus, 5 mm/min: 3350 MPa (ASTM D638)
  • Flexural Stress at Yield, 1.3 mm/min, 50 mm Span: 165 MPa (ASTM D790)
  • Flexural Modulus, 1.3 mm/min, 50 mm Span: 3200 MPa (ASTM D790)
  • Flexural Stress at Yield, 2.6 mm/min, 100 mm Span: 160 MPa (ASTM D790)
  • Flexural Modulus, 2.6 mm/min, 100 mm Span: 3400 MPa (ASTM D790)
  • Rockwell Hardness: M109 (ASTM D785)
  • Taber Abrasion, CS-17, 1 kg: 10 mg/1000 cycles (ASTM D1044)
Impact Properties
  • Izod Impact, Unnotched, 80 × 10 × 4 mm, 23°C: NB (ISO 180/1U)
  • Izod Impact, Unnotched, 80 × 10 × 4 mm, -30°C: NB (ISO 180/1U)
  • Izod Impact, Unnotched, 23°C: 1600 J/m (ASTM D4812)
  • Izod Impact, Unnotched, -30°C: 1500 J/m (ASTM D4812)
  • Izod Impact, Notched, 80 × 10 × 4 mm, 23°C: 5 kJ/m² (ISO 180/1A)
  • Izod Impact, Notched, 80 × 10 × 4 mm, -30°C: 5 kJ/m² (ISO 180/1A)
  • Izod Impact, Notched, 23°C: 32 J/m (ASTM D256)
  • Izod Impact, Notched, -30°C: 41 J/m (ASTM D256)
  • Charpy Impact, V-Notch Edgewise, 23°C: 4 kJ/m² (ISO 179/1eA)
  • Charpy Impact, V-Notch Edgewise, -30°C: 4 kJ/m² (ISO 179/1eA)
  • Izod Impact, Reverse Notched, 3.2 mm: 1174 J/m (ASTM D256)
  • Gardner Impact, 23°C: 33 J (SABIC Method)
Thermal Properties
  • Glass Transition Temperature, Tg: 217°C (SABIC Datasheet Description)
  • HDT/Bf, 0.45 MPa, Flatwise, 80 × 10 × 4 mm: 209°C (ISO 75/Bf)
  • HDT/Af, 1.8 MPa, Flatwise, 80 × 10 × 4 mm: 192°C (ISO 75/Af)
  • Vicat Softening Temperature, Rate A/50: 215°C (ISO 306)
  • Vicat Softening Temperature, Rate B/50: 211°C (ISO 306)
  • Vicat Softening Temperature, Rate B/120: 212°C (ISO 306)
  • CTE, -40°C to 150°C, Flow: 5.2E-05 1/°C (ISO 11359-2)
  • CTE, -40°C to 150°C, Cross Flow: 5.2E-05 1/°C (ISO 11359-2)
  • Ball Pressure Test, 125°C ± 2°C: PASS (IEC 60695-10-2)
  • Thermal Conductivity: 0.22 W/m-°C (ISO 8302)
  • HDT, 0.45 MPa, 6.4 mm, Unannealed: 210°C (ASTM D648)
  • HDT, 1.82 MPa, 6.4 mm, Unannealed: 201°C (ASTM D648)
  • HDT, 0.45 MPa, 3.2 mm, Unannealed: 207°C (ASTM D648)
  • HDT, 1.82 MPa, 3.2 mm, Unannealed: 190°C (ASTM D648)
  • Vicat Softening Temperature, Rate B/50: 211°C (ASTM D1525)
  • CTE, -20°C to 150°C, Flow: 5.2E-05 1/°C (ASTM E831)
  • CTE, -20°C to 150°C, Cross Flow: 5.2E-05 1/°C (ASTM E831)
  • Thermal Conductivity: 0.22 W/m-°C (ASTM C177)
Electrical Properties
  • Volume Resistivity: 1.E+15 Ω·cm (IEC 60093)
  • Surface Resistivity, ROA: >1.E+15 Ω (IEC 60093)
  • Dielectric Strength, in Oil, 0.8 mm: 33 kV/mm (IEC 60243-1)
  • Dielectric Strength, in Oil, 1.6 mm: 25 kV/mm (IEC 60243-1)
  • Dielectric Strength, in Oil, 3.2 mm: 16 kV/mm (IEC 60243-1)
  • Relative Permittivity, 1 MHz: 2.9 (IEC 60250)
  • Dissipation Factor, 50/60 Hz: 0.0005 (IEC 60250)
  • Dissipation Factor, 1 MHz: 0.006 (IEC 60250)
  • Relative Permittivity, 50/60 Hz: 2.9 (IEC 60250)
  • Comparative Tracking Index: 150 V (IEC 60112)
  • Comparative Tracking Index, M: 100 V (IEC 601112)
  • Volume Resistivity: 1.E+17 Ω·cm (ASTM D257)
  • Dielectric Strength, in Air, 1.6 mm: 32.7 kV/mm (ASTM D149)
  • Dielectric Strength, in Oil, 1.6 mm: 28.0 kV/mm (ASTM D149)
  • Dielectric Strength, in Oil, 3.2 mm: 19.7 kV/mm (ASTM D149)
  • Relative Permittivity, 100 Hz: 3.15 (ASTM D150)
  • Relative Permittivity, 1 kHz: 3.15 (ASTM D150)
  • Dissipation Factor, 100 Hz: 0.0015 (ASTM D150)
  • Dissipation Factor, 1 kHz: 0.0012 (ASTM D150)
Flame Characteristics
  • UL Flame Class Rating, 94V-0: 0.71 mm (UL 94 by SABIC-IP)
  • UL 94-5VA Rating: 3 mm (UL 94 by SABIC-IP)
  • Glow Wire Flammability Index, 960°C: Passes at 3.2 mm (IEC 60695-2-12)
  • Oxygen Index, LOI: 47% (ISO 4589)
  • Oxygen Index, LOI: 44% (ASTM D2863)
  • NBS Smoke Density, Flaming, Ds 4 min: 2 (ASTM E662)
Processing Parameters
  • Drying Temperature: 150°C
  • Drying Time: 4–6 hrs
  • Cumulative Drying Time: 24 hrs
  • Maximum Moisture Content: 0.02%
  • Melt Temperature: 350–410°C
  • Nozzle Temperature: 345–405°C
  • Front Zone 3 Temperature: 345–415°C
  • Middle Zone 2 Temperature: 340–405°C
  • Rear Zone 1 Temperature: 330–400°C
  • Mold Temperature: 135–180°C
  • Back Pressure: 0.3–0.7 MPa
  • Screw Speed, Circumferential Speed: 0.2–0.3 m/s
  • Shot to Cylinder Size: 40–60%
  • Vent Depth: 0.025–0.076 mm

Use & Applications

  • Automotive
  • building & construction
  • consumer
  • E&E
  • healthcare
  • industrial
  • mass transportation
  • packaging
sabic ultem pei resin 25kg package

Send Us a Message

Please enter your query and share a few details, and we will get back to you shortly.