Plastic Granules
ULTEM™ Resin 1010P200
ULTEM™ Resin 1010P200 is an unreinforced amorphous PEI powder with D50 200 micron particle size. It offers Tg 217°C, high flow, flame resistance, and strong electrical insulation. It supports sintering, powder coating, and composite impregnation for high-temperature parts.
Associated Documents
TDS - Global
Typical property data
Physical Properties
- Particle Size D50: 200 micron
- Particle Size D100: 450 micron
- Density: 1.27 g/cm³ (ISO 1183)
- Specific Gravity: 1.27 (ASTM D792)
- Moisture Absorption, 23°C / 50% RH / 24 hrs: 0.2% (ISO 62-4)
- Moisture Absorption, 23°C / 50% RH / Equilibrium: 0.7% (ISO 62-4)
- Water Absorption, 23°C / 24 hrs: 0.25% (ISO 62-1)
- Water Absorption, 23°C / Saturated: 1.25% (ISO 62-1)
- Water Absorption, 23°C / 24 hrs: 0.25% (ASTM D570)
- Water Absorption, 23°C / Saturated: 1.25% (ASTM D570)
- Melt Volume Rate, 360°C / 5.0 kg: 25 cm³/10 min (ISO 1133)
- Melt Volume Rate, 340°C / 5.0 kg: 13 cm³/10 min (ISO 1133)
- Melt Flow Rate, 337°C / 6.6 kgf: 17.8 g/10 min (ASTM D1238)
- Poisson’s Ratio: 0.36 (ASTM E132)
Mechanical Properties
- Tensile Stress, Yield, 50 mm/min: 110 MPa (ISO 527)
- Tensile Strain, Yield, 50 mm/min: 6% (ISO 527)
- Tensile Strain, Break, 50 mm/min: 50% (ISO 527)
- Tensile Modulus, 1 mm/min: 3200 MPa (ISO 527)
- Flexural Stress, Yield, 2 mm/min: 160 MPa (ISO 178)
- Flexural Modulus, 2 mm/min: 3300 MPa (ISO 178)
- Ball Indentation Hardness, H358/30: 140 MPa (ISO 2039-1)
- Rockwell Hardness: M106 (ISO 2039-2)
- Tensile Stress, Yield, Type I, 50 mm/min: 115 MPa (ASTM D638)
- Tensile Strain, Yield, Type I, 50 mm/min: 7% (ASTM D638)
- Tensile Strain, Break, Type I, 50 mm/min: 60% (ASTM D638)
- Tensile Stress, Yield, Type I, 5 mm/min: 110 MPa (ASTM D638)
- Tensile Strain, Yield, Type I, 5 mm/min: 7% (ASTM D638)
- Tensile Strain, Break, Type I, 5 mm/min: 60% (ASTM D638)
- Tensile Modulus, 5 mm/min: 3350 MPa (ASTM D638)
- Flexural Stress, Yield, 1.3 mm/min, 50 mm Span: 165 MPa (ASTM D790)
- Flexural Modulus, 1.3 mm/min, 50 mm Span: 3200 MPa (ASTM D790)
- Flexural Stress, Yield, 2.6 mm/min, 100 mm Span: 160 MPa (ASTM D790)
- Flexural Modulus, 2.6 mm/min, 100 mm Span: 3400 MPa (ASTM D790)
- Rockwell Hardness: M109 (ASTM D785)
- Taber Abrasion, CS-17, 1 kg: 10 mg/1000 cycles (ASTM D1044)
Impact Properties
- Izod Impact, Reverse Notched, 3.2 mm: 1174 J/m (ASTM D256)
- Gardner Impact, 23°C: 33 J (SABIC Method)
- Izod Impact, Unnotched, 80 × 10 × 4 mm, +23°C: NB (ISO 180/1U)
- Izod Impact, Unnotched, 80 × 10 × 4 mm, -30°C: NB (ISO 180/1U)
- Izod Impact, Unnotched, 23°C: 1600 J/m (ASTM D4812)
- Izod Impact, Unnotched, -30°C: 1500 J/m (ASTM D4812)
- Izod Impact, Notched, 80 × 10 × 4 mm, +23°C: 5 kJ/m² (ISO 180/1A)
- Izod Impact, Notched, 80 × 10 × 4 mm, -30°C: 5 kJ/m² (ISO 180/1A)
- Izod Impact, Notched, 23°C: 32 J/m (ASTM D256)
- Izod Impact, Notched, -30°C: 41 J/m (ASTM D256)
- Charpy Impact, 23°C, V-Notch Edgewise, 80 × 10 × 4 mm, Span 62 mm: 4 kJ/m² (ISO 179/1eA)
- Charpy Impact, -30°C, V-Notch Edgewise, 80 × 10 × 4 mm, Span 62 mm: 4 kJ/m² (ISO 179/1eA)
Thermal Properties
- Glass Transition Temperature, Tg: 217°C
- HDT/Bf, 0.45 MPa, Flatwise, 80 × 10 × 4 mm, Span 64 mm: 209°C (ISO 75/Bf)
- HDT/Af, 1.8 MPa, Flatwise, 80 × 10 × 4 mm, Span 64 mm: 192°C (ISO 75/Af)
- Vicat Softening Temperature, Rate A/50: 215°C (ISO 306)
- Vicat Softening Temperature, Rate B/50: 211°C (ISO 306)
- Vicat Softening Temperature, Rate B/120: 212°C (ISO 306)
- CTE, -40°C to 150°C, Flow: 5.2E-05 1/°C (ISO 11359-2)
- CTE, -40°C to 150°C, Cross Flow: 5.2E-05 1/°C (ISO 11359-2)
- Ball Pressure Test, 125°C ± 2°C: PASS (IEC 60695-10-2)
- Thermal Conductivity: 0.22 W/m-°C (ISO 8302)
- HDT, 0.45 MPa, 6.4 mm, Unannealed: 210°C (ASTM D648)
- HDT, 1.82 MPa, 6.4 mm, Unannealed: 201°C (ASTM D648)
- HDT, 0.45 MPa, 3.2 mm, Unannealed: 207°C (ASTM D648)
- HDT, 1.82 MPa, 3.2 mm, Unannealed: 190°C (ASTM D648)
- Vicat Softening Temperature, Rate B/50: 211°C (ASTM D1525)
- CTE, -20°C to 150°C, Flow: 5.6E-05 1/°C (ASTM E831)
- CTE, -20°C to 150°C, Cross Flow: 5.4E-05 1/°C (ASTM E831)
- Thermal Conductivity: 0.22 W/m-°C (ASTM C177)
Electrical Properties
- Volume Resistivity: 1.E+15 Ω·cm (IEC 60093)
- Surface Resistivity, ROA: >1.E+15 Ω (IEC 60093)
- Dielectric Strength, In Oil, 0.8 mm: 33 kV/mm (IEC 60243-1)
- Dielectric Strength, In Oil, 1.6 mm: 25 kV/mm (IEC 60243-1)
- Dielectric Strength, In Oil, 3.2 mm: 16 kV/mm (IEC 60243-1)
- Relative Permittivity, 1 MHz: 2.9 (IEC 60250)
- Relative Permittivity, 50/60 Hz: 2.9 (IEC 60250)
- Dissipation Factor, 50/60 Hz: 0.0005 (IEC 60250)
- Dissipation Factor, 1 MHz: 0.006 (IEC 60250)
- Dissipation Factor, 1.1 GHz: 0.0012
- Dissipation Factor, 5 GHz: 0.0024
- Dissipation Factor, 10 GHz: 0.0027
- Dissipation Factor, 100 Hz: 0.0015 (ASTM D150)
- Dissipation Factor, 1 kHz: 0.0012 (ASTM D150)
- Dielectric Constant, 1.1 GHz: 3.01
- Dielectric Constant, 5 GHz: 3.02
- Dielectric Constant, 10 GHz: 3.02
- Comparative Tracking Index: 150 V (IEC 60112)
- Comparative Tracking Index, M: 100 V (IEC 60112)
- Volume Resistivity: 1.E+17 Ω·cm (ASTM D257)
- Dielectric Strength, In Air, 1.6 mm: 32.7 kV/mm (ASTM D149)
- Dielectric Strength, In Oil, 1.6 mm: 28.0 kV/mm (ASTM D149)
- Dielectric Strength, In Oil, 3.2 mm: 19.7 kV/mm (ASTM D149)
- Relative Permittivity, 100 Hz: 3.15 (ASTM D150)
- Relative Permittivity, 1 kHz: 3.15 (ASTM D150)
Flame Characteristics
- Oxygen Index, LOI: 44% (ASTM D2863)
- Oxygen Index, LOI: 47% (ISO 4589)
- Flame Retardant Type: Inherently flame retardant
- Flame Retardant System: Non-halogenated flame retardant
Processing Parameters
- Processing Techniques: Sintering, Powder Coating, Impregnation for composites
- Powder Average Particle Size, D50: 200 micron
- Powder Maximum Particle Size, D100: 450 micron
- Melt Volume Rate, 360°C / 5.0 kg: 25 cm³/10 min (ISO 1133)
- Melt Volume Rate, 340°C / 5.0 kg: 13 cm³/10 min (ISO 1133)
- Melt Flow Rate, 337°C / 6.6 kgf: 17.8 g/10 min (ASTM D1238)
Use & Applications
- Automotive
- building & construction
- consumer
- E&E
- industrial
- mass transportation
- packaging